Welding Procedure Qualification Certificate (EN ISO 15614-1) · This is a copy of an electronic...

13
Lloyd's Register Group Limited, its affiliates and subsidiaries and their respective officers, employees or agents are, individually and collectively, referred to in this clause as 'Lloyd's Register'. Lloyd's Register assumes no responsibility and shall not be liable to any person for any loss, damage or expense caused by reliance on the information or advice in this document or howsoever provided, unless that person has signed a contract with the relevant Lloyd's Register entity for the provision of this information or advice and in that case any responsibility or liability is exclusively on the terms and conditions set out in that contract. Form 4102 (2013.12) Certificate no: HAM 1571024/2 Page 1 of Welding Procedure Qualification Certificate (EN ISO 15614-1) Energy - Downstream, Power and Manufacturing Manufacturer’s Welding Procedure Qualification Record No.: VP16E Examining body Reference No: / Manufacturer: Ruhfus Systemhydraulik GmbH Address: Neuss / Germany Welders Name Jacek Nakonieczny Code/Testing Standard: EN ISO 15614, Lloyd's Register Rules and Regulations Date of Welding: 22 May 2015 Range of Qualification Welding Process(es): 141 (TIG) Type of joint and weld: V-Joint 40°-60° Parent material group(s) and sub- () 8.1 / 8.1 Parent Material Thickness (mm): 4,0 Weld Metal Thickness (mm): 4,0 Throat Thickness (mm) 2,0-3,5 Single Run/Multi Run Multi Run Outside Pipe Diameter (mm): 30,0 Filler Material Designation: Thermanit GE-316 L Filler Material Make: Böhler Filler Material Size: Ø 2,0 mm Designation of Shielding Gas/Flux: EN ISO 14175-I1-Ar Designation of Backing Gas: EN ISO 14175-I1-Ar Type of Welding Current and Polarity: direct current (-) Mode of Metal Transfer: --- Heat Input: 0,4-1,08 kJ/mm Welding Positions: PC+PF Preheat Temperature: 15,0°C Interpass Temperature: 150,0°C Post-Heating: --- Post-Weld Heat Treatment and/or A i --- Other Information For further details see WPS VO16E PC+PH and Techno Labor test report. Certified that test welds were prepared, welded and tested satisfactorily in accordance with the requirements of the code/testing standard indicated above. Location: Dortmund Date of Issue: 18 June 2015 Surveyor For K. Nebel: Surveyor to Lloyd's Register EMEA A subsidiary of Lloyd's Register Group Limited Examining Body

Transcript of Welding Procedure Qualification Certificate (EN ISO 15614-1) · This is a copy of an electronic...

Page 1: Welding Procedure Qualification Certificate (EN ISO 15614-1) · This is a copy of an electronic document. In the event of any conflict or ambiguity between the copy and the electronic

This is a copy of an electronic document. In the event of any conflict or ambiguity between the copy and the electronic document,which is retained and published by Lloyd's Register, the original electronic and certified version shall always prevail.

Lloyd's Register Group Limited, its affiliates and subsidiaries and their respective officers, employees or agents are, individually and collectively, referred to in this clause as 'Lloyd's Register'. Lloyd's Register assumes no responsibility and shall not be liable to any person for any loss, damage or expense caused by reliance on the information or advice in this document or howsoever provided, unless that person has signed a contract with the relevant Lloyd's Register entity for the provision of this information or advice and in that case any responsibility or liability is exclusively on the terms and conditions set out in that contract.

Form 4102 (2013.12)

Certificate no: HAM 1571024/2 Page 1 of -

Welding Procedure Qualification Certificate (EN ISO 15614-1) Energy - Downstream, Power and Manufacturing

Manufacturer’s Welding Procedure Qualification Record No.:

VP16E Examining body Reference No:

/

Manufacturer: Ruhfus Systemhydraulik GmbH Address: Neuss / Germany

Welders Name Jacek Nakonieczny Code/Testing Standard: EN ISO 15614, Lloyd's Register Rules and Regulations

Date of Welding: 22 May 2015 Range of Qualification

Welding Process(es): 141 (TIG)

Type of joint and weld: V-Joint 40°-60° Parent material group(s) and sub-

( ) 8.1 / 8.1

Parent Material Thickness (mm): 4,0

Weld Metal Thickness (mm): 4,0

Throat Thickness (mm) 2,0-3,5

Single Run/Multi Run Multi Run

Outside Pipe Diameter (mm): 30,0

Filler Material Designation: Thermanit GE-316 L

Filler Material Make: Böhler

Filler Material Size: Ø 2,0 mm

Designation of Shielding Gas/Flux: EN ISO 14175-I1-Ar

Designation of Backing Gas: EN ISO 14175-I1-Ar

Type of Welding Current and Polarity: direct current (-)

Mode of Metal Transfer: ---

Heat Input: 0,4-1,08 kJ/mm

Welding Positions: PC+PF

Preheat Temperature: ≥15,0°C

Interpass Temperature: ≥150,0°C

Post-Heating: --- Post-Weld Heat Treatment and/or A i

---

Other Information For further details see WPS VO16E PC+PH and Techno Labor test report.

Certified that test welds were prepared, welded and tested satisfactorily in accordance with the requirements of the code/testing standard indicated above. Location: Dortmund Date of Issue: 18 June 2015

Surveyor

For K. Nebel:

Surveyor to Lloyd's Register EMEA

A subsidiary of Lloyd's Register Group Limited

Examining Body

BMNTAS
LR031.1.2013.12
Page 2: Welding Procedure Qualification Certificate (EN ISO 15614-1) · This is a copy of an electronic document. In the event of any conflict or ambiguity between the copy and the electronic
Page 3: Welding Procedure Qualification Certificate (EN ISO 15614-1) · This is a copy of an electronic document. In the event of any conflict or ambiguity between the copy and the electronic
Page 4: Welding Procedure Qualification Certificate (EN ISO 15614-1) · This is a copy of an electronic document. In the event of any conflict or ambiguity between the copy and the electronic
Page 5: Welding Procedure Qualification Certificate (EN ISO 15614-1) · This is a copy of an electronic document. In the event of any conflict or ambiguity between the copy and the electronic
Page 6: Welding Procedure Qualification Certificate (EN ISO 15614-1) · This is a copy of an electronic document. In the event of any conflict or ambiguity between the copy and the electronic
Page 7: Welding Procedure Qualification Certificate (EN ISO 15614-1) · This is a copy of an electronic document. In the event of any conflict or ambiguity between the copy and the electronic
Page 8: Welding Procedure Qualification Certificate (EN ISO 15614-1) · This is a copy of an electronic document. In the event of any conflict or ambiguity between the copy and the electronic
Page 9: Welding Procedure Qualification Certificate (EN ISO 15614-1) · This is a copy of an electronic document. In the event of any conflict or ambiguity between the copy and the electronic
Page 10: Welding Procedure Qualification Certificate (EN ISO 15614-1) · This is a copy of an electronic document. In the event of any conflict or ambiguity between the copy and the electronic
Page 11: Welding Procedure Qualification Certificate (EN ISO 15614-1) · This is a copy of an electronic document. In the event of any conflict or ambiguity between the copy and the electronic
Page 12: Welding Procedure Qualification Certificate (EN ISO 15614-1) · This is a copy of an electronic document. In the event of any conflict or ambiguity between the copy and the electronic
Page 13: Welding Procedure Qualification Certificate (EN ISO 15614-1) · This is a copy of an electronic document. In the event of any conflict or ambiguity between the copy and the electronic