![Page 1: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/1.jpg)
1
Casting2.810Prof. Timothy Gutowski
![Page 2: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/2.jpg)
2
Casting since about 4000 BC…
Ancient Greece; bronzestatue casting circa 450BC
Iron works in early Europe,e.g. cast iron cannons fromEngland circa 1543
![Page 3: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/3.jpg)
3
OutlineSand Casting, Investment Casting, Die CastingBasics and countermeasuresPhase Change, ShrinkageHeat TransferPattern DesignVariations & DevelopmentsEnvironmental Issues
![Page 4: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/4.jpg)
4
CastingReadings;1. Kalpakjian, Chapters 10,
11, 122. Booothroyd, “Design for
Die Casting”3. Flemings “Heat Flow in
Solidification”
Note: a good heat transfer reference can be found by Prof John Lienhard online http://web.mit.edu/lienhard/www/ahtt.html
![Page 5: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/5.jpg)
5
Casting Methods
• Sand CastingHigh Temperature Alloy, Complex Geometry, Rough Surface Finish
• Investment CastingHigh Temperature Alloy, Complex Geometry, Moderately Smooth Surface Finish
• Die CastingHigh Temperature Alloy, Moderate Geometry, Smooth Surface
![Page 6: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/6.jpg)
6
Sand Casting
![Page 7: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/7.jpg)
7
Sand CastingDescription: Tempered sand is packed into wood or metal pattern halves, removed form the pattern, and assembled with or without cores, and metal is poured into resultant cavities. Various core materials can be used. Molds are broken to remove castings. Specialized binders now in use can improve tolerances and surface finish.Metals: Most castable metals.Size Range: Limitation depends on foundry capabilities. Ounces to many tons.Tolerances:
Non-Ferrous 1/32 to 6 Add .003 to 3, 3/64 from 3 to 6.Across parting line add .020 to .090 depending on size. (Assumes metal patterns)
Surface Finish:Non-Ferrous: 150-350 RMSFerrous: 300-700RMS
Minimum Draft Requirements:1° to 5°Cores: 1° to 1 1/2°
Normal Minimum Section Thickness:Non-Ferrous: 1/8 - 1/4 Ferrous: 1/4 - 3/8
Ordering Quantities: All quantitiesNormal Lead Time:
Samples: 2-10 weeksProduction 2-4 weeks A.S.A.
![Page 8: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/8.jpg)
8
Sand Casting Mold Features
Vents, which are placed in molds to carry off gases produced when the molten metal comes into contact with the sand in the molds and core. They also exhaust air from the mold cavity as the molten metal flows into the mold.
![Page 9: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/9.jpg)
9
See Video from Mass Foundry
![Page 10: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/10.jpg)
10
Production sand casting
![Page 11: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/11.jpg)
11
Investment Casting
The investment-casting process, also called the lost-wax process, was first used during the period 4000-3500 B.C. The pattern is made of wax or a plastic such as polystyrene. The sequences involved in investment casting are shown in Figure 11.18. The pattern is made by injecting molten wax or plastic into a metal die in the shape of the object.
![Page 12: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/12.jpg)
12
Investment CastingDescription: Metal mold makes wax or plastic replica. There are sprued, then surrounded with investment material, baked out, and metal is poured in the resultant cavity. Molds are broken to remove the castings.Metals: Most castable metals.Size Range: fraction of an ounce to 150 lbs..Tolerances:
.003 to 1/4 .004 to 1/2, .005 per inch to 3 .003 for each additional inch
Surface Finish:63-125RMS
Minimum Draft Requirements: NoneNormal Minimum Section Thickness:
.030 (Small Areas)
.060 (Large Areas)Ordering Quantities:
Aluminum: usually under 1,000Other metals: all quantities
Normal Lead Time:Samples: 5-16 weeks (depending on complexity)Production 4-12 weeks A.S.A. (depending on subsequent operations).
Talbot Associates Inc.
![Page 13: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/13.jpg)
13
Die Casting – Cold-Chamber Casting
Cycle in cold-chamber casting: (1) with die closed and ram withdrawn, molten metal is poured into the chamber; (2) ram forces metal to flow into die, maintaining pressure during the cooling and solidification; and (3) ram is withdrawn, die is opened, and part is ejected. Used for higher temperature metals eg Aluminum, Copper and alloys
![Page 14: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/14.jpg)
14
Die Casting – Hot-Chamber Casting
Cycle in hot-chamber casting: (1) with die closed and plunger withdrawn, molten metal flows into the chamber; (2) plunger forces metal in chamber to flow into die, maintaining pressure during cooling and solidification; and (3) plunger is withdrawn, die is opened, and solidified part is ejected. Finished part is shown in (4).
![Page 15: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/15.jpg)
15
Die CastingDescription: Molten metal is injected, under pressure, into hardened steel dies, often water cooled. Dies are opened, and castings are ejected.Metals: Aluminum, Zinc, Magnesium, and limited Brass.Size Range: Not normally over 2 feet square. Some foundries capable of larger sizes.Tolerances:
Al and Mg .002/in.Zinc .0015/in. Brass .001/in.Add .001 to .015 across parting line depending on size
Surface Finish: 32-63RMSMinimum Draft Requirements:
Al & Mg: 1° to 3°Zinc: 1/2° to 2°Brass: 2° to 5°
Normal Minimum Section Thickness:Al & Mg: .03 Small Parts: .06 Medium Parts Zinc: .03 Small Parts: .045 Medium Parts Brass: .025 Small Parts: .040 Medium Parts
Ordering Quantities: Usually 2,500 and up.
Normal Lead Time:Samples: 12-20 weeks Production: ASAP after approval.
![Page 16: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/16.jpg)
16
High Melt Temperature•Chemical Activity•High Latent Heat•Handling•Off-gassing
3000° C
0° C
1000° C
2000° C
Tungsten Carbide, WC, Silicon Carbide, SiC
Molybdenum
Alumina Al2O3
Platinum, PtTitanium, TiIronFE, Plain Carbon Steels, low alloy, stainlessNickel, NiNickel Allows
Cubic Zirconia, ZrO2
Silicon, Si
Copper, Cu, Bronze, Brass
AluminumMagnesiumZinc, ZnPTFE (Teflon)Tin, SnHDPE
NylonAcetal
![Page 17: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/17.jpg)
17
Mold FillingBernouli’s Equation:
Reynold’s Number:
•Short filling times•Potential Turbulence(see p. 273 … Kalpakjian
.2
2
Constgv
pgph
vDP
Re
h
![Page 18: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/18.jpg)
18
Mold Filling Example (1 of 2)
![Page 19: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/19.jpg)
19
Mold Filling Example (2 of 2)
![Page 20: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/20.jpg)
20
PhaseChange &Shrinkage
![Page 21: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/21.jpg)
21
Solidification of a binary alloy
![Page 22: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/22.jpg)
22
Composition change during solidification
![Page 23: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/23.jpg)
23
Solidification
![Page 24: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/24.jpg)
24
Cast structuresSchematic illustration of three cast structures solidified in a square mold: (a) pure metals; (b) solid solution alloys; and © structure obtained by using nucleating agents. Source: G. W. Form, J. F. Wallace, and A. Cibula
![Page 25: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/25.jpg)
25
Pop quiz; If you top fill the mold below, what will the part look like after solidification?
![Page 26: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/26.jpg)
26
Can you explain these features?
![Page 27: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/27.jpg)
27
Heat Transfer – Sand Casting
2
AVt s
![Page 28: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/28.jpg)
28
Heat Transfer – Die Casting
1
AVt s
![Page 29: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/29.jpg)
29
Steady State Conduction Heat Transfer
Figure 1
![Page 30: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/30.jpg)
30
Steady State Conduction Heat Transfer
Figure 2
![Page 31: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/31.jpg)
31
Thermal Conductivity “k” of Various Materials for Parts and Molds (W/m °K)
Copper 394Aluminum 222Iron 29Sand 0.61PMMA 0.20PVC 0.16
dxdTkq
![Page 32: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/32.jpg)
32
Film Coefficients W/m2°KTypical die casting 5,000Natural convection 1 - 10Flowing air 10 - 50
Thq
![Page 33: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/33.jpg)
33
Transient Heat Transfer
![Page 34: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/34.jpg)
34
Sand Casting (see Flemings)
![Page 35: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/35.jpg)
35
Sand Casting (see Flemings)
![Page 36: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/36.jpg)
36
Solidification Time
enthapy
Use Flemings result here
![Page 37: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/37.jpg)
37
Solidification Time (cont.)
![Page 38: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/38.jpg)
38
Cooling Time; thin slab
![Page 39: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/39.jpg)
39
Cooling time;intersection
1
1211
2hL
hAV
![Page 40: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/40.jpg)
40
Pattern Design suggestions
![Page 41: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/41.jpg)
41
More PatternDesignsuggestions
![Page 42: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/42.jpg)
42
And more…Figure 7.2.32Omit outside bosses and the need for cores.(Courtesy of Meehanite Metal Corp.)
Figure 7.2.35Avoid using ribs which meet at acute angles.(Courtesy of Meehanite Metal Corp.)
![Page 43: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/43.jpg)
43
Die Casting SolidificationTime
s
Time to form solid part A
![Page 44: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/44.jpg)
44
Time to cool part to the ejection temperature. (lumped parameter model)
mCp
dTdt
Ah T To
let T To
tf
tip
dtmCAhdi
f
i = Ti + Tsp - Tmold Tsp = H/Cp f = Teject - Tmold
t mCpAh
ln fi
Integration yields…
t
wCp2h ln
TinjectTsp TmoldTeject Tmold
Or for thin sheets of thickness “w”,
“sp” means superheat
![Page 45: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/45.jpg)
45
Pattern Design Issues (Alum)
Shrinkage Allowance .013/1Machining Allowance 1/16”Minimum thickness 3/16”Parting LineDraft Angle 3 to 5%Uniform Thickness
![Page 46: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/46.jpg)
46
Pattern DesignTable 12.1Normal Shrinkage Allowance for Some Metals Cast in Sand MoldsMetal PercentGray cast iron0.83 – 1.3White cast iron 2.1Malleable cast iron0.78 – 1.0Aluminum alloys 1.3Magnesium alloys 1.3Yellow brass 1.3 – 1.6Phosphor bronze1.0 – 1.6Aluminum bronze 2.1High-manganese steel2.6
![Page 47: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/47.jpg)
47
Variations and Developments
Continuous castingLost foam molding3D Printing of Investment toolingDirect printing with metal dropletsUniform metal spray
![Page 48: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/48.jpg)
48
Continuous casting ref AISI
Steel from the electric or basic oxygen furnace is tapped into a ladle and taken to the continuous casting machine. The ladle is raised onto a turret that rotates the ladle into the casting position above the tundish. Referring to Figure 2, liquid steel flows out of the ladle (1) into the tundish (2), and then into a water-cooled copper mold (3). Solidification begins in the mold, and continues through the First Zone (4) and Strand Guide (5). In this configuration, the strand is straightened (6), torch-cut (8), then discharged (12) for intermediate storage or hot charged for finished rolling.
![Page 49: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/49.jpg)
49
3D Printingof Investment cast tooling
Spread PowderLayer
Print Selected Area Lower Piston
Completed PartsLast Layer Printed
![Page 50: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/50.jpg)
50
Shell and part (Turbine blade)
![Page 51: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/51.jpg)
51
Microcasting of droplets
CMU MIT
![Page 52: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/52.jpg)
52
Environmental IssuesSmeltingEnergyOff-gassing see AFS webpage on green sand emissions; http://www.afsinc.org/environmental.html
Cooling waterWaste sand disposalOff shore locations
![Page 53: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/53.jpg)
53
Metal Smelting; reducing oxides and sulfides to metal…..
http://www.steel.org/learning/howmade/blast_furnace.htm
![Page 54: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/54.jpg)
54
Environmental loads by manufacturing sectorCarbon Dioxide and Toxic Materials per Value of Shipments
00.5
11.5
22.5
33.5
44.5
5
Che
mic
als
Pet
role
uman
d C
oal
Pla
stic
s an
dR
ubbe
r
Prim
ary
Met
al
Fabr
icat
edM
etal
Mac
hine
ry
Ele
ctro
nic
Tran
spor
tatio
n Manufacturing industries
Wei
ght/D
olla
rs
CO2 (metric ton/$10,000)
Toxic Mat'ls (lb/$1000)
EPA 2001, DOE 2001
![Page 55: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/55.jpg)
55
The estimated environmental performance of various mfg processes (not including auxiliary requirements)
*Energy per wt. normalizedby the melt energy ** total raw mat’l normalized
by the part wt.
![Page 56: Casting 091213101224-phpapp02](https://reader034.fdocuments.in/reader034/viewer/2022051608/540530e08d7f729e768b4b10/html5/thumbnails/56.jpg)
56
SummarySand Casting, Investment Casting, Die Casting
Basics and countermeasuresPhase Change, ShrinkageHeat TransferPattern DesignVariations and DevelopmentsEnvironmental Issues