Available online at www.sciencedirect.com
www.elsevier.com/locate/cma
Comput. Methods Appl. Mech. Engrg. 197 (2008) 3174–3181
Simulating nanoindentation and predicting dislocation nucleationusing interatomic potential finite element method
Yuan Zhong, Ting Zhu *
Woodruff School of Mechanical Engineering, Georgia Institute of Technology, Atlanta, GA 30032, USA
Received 7 September 2007; received in revised form 23 September 2007; accepted 8 October 2007Available online 26 December 2007
Abstract
Dislocation nucleation is central to our understanding of the onset of plasticity during nanoindentation. The shear stress in smallvolumes beneath the nanoindenter can achieve the theoretical limit of a perfect crystal. The ensuing nonlinear elastic instability can trig-ger homogenous dislocation nucleation inside the crystal. Here we employ the interatomic potential finite element method to simulatenanoindentation and predict dislocation nucleation. Simulations are performed for indentation on the (111), (110) and (100) surfacesof Al, Cu, Ni single crystals. We quantify the critical conditions of dislocation nucleation, including the indentation load of nucleation,location of nucleation site, nucleation stress and activated slip system. We find these conditions sensitively depend on indentation ori-entation, but are consistent for different crystals. The results highlight the critical role of hyperelasticity (the nonlinear elasticity causedby elastic softening at large strain) and crystallography in dislocation nucleation in small material volumes. Our study also reveals thedeficiency of commonly used nucleation criterion such as the critical resolved shear stress.� 2007 Elsevier B.V. All rights reserved.
Keywords: Interatomic potential finite element method; Nanoindentation; Dislocation nucleation
1. Introduction
In nanoindentation experiments, the shear stress at theonset of plasticity can approach the theoretical shearstrength of a perfect crystal [1–6]. Such ultra-high stressoccurs in small (nanometer-sized) volumes beneath thenanoindenter, which can be free of any pre-existing defects.A defect-free crystal deforms in a nonlinear manner, whenthe shear stress approaches the theoretical limit. The non-linear elastic, or the so-called hyperelastic, response arisesfrom the elastic softening of crystal lattice at large strain.This paper is concerned with the critical role of hyperelas-ticity, as well as crystallography, in the onset of plasticityduring nanoindentation, a process arguably associatedwith homogenous dislocation nucleation that result fromthe nonlinear elastic instability of crystal at large shear.
0045-7825/$ - see front matter � 2007 Elsevier B.V. All rights reserved.
doi:10.1016/j.cma.2007.10.009
* Corresponding author. Tel.: +1 404 894 6597.E-mail address: [email protected] (T. Zhu).
Here we employ the interatomic potential finite elementmethod (IPFEM) [7–9] to simulate nanoindentation andpredict homogenous dislocation nucleation. The IPFEMsimulation takes as an input the interatomic potential-based constitutive relation derived within the frameworkof hyperelasticity of single crystals [10]. It can accuratelycapture the essential physical effects of crystal at largedeformation: nonlinear elasticity and shear asymmetry(i.e., the asymmetry of shear stress with respect to thesense of shearing in the Shockley partial direction off111gh11�2i), thereby enabling an accurate prediction ofdislocation nucleation. Compared to the commonly usedmolecular dynamics (MD), the IPFEM significantlyimproves the computational efficiency, so that the effectsof system size and loading rate can be minimized, and con-sequently simulations of nanoindentation can be per-formed on the length and time scales close to laboratoryexperiments.
In this study, simulations are performed for nanoinden-tation on several face-centered cubic (fcc) crystals at low
Y. Zhong, T. Zhu / Comput. Methods Appl. Mech. Engrg. 197 (2008) 3174–3181 3175
temperature (nearly zero-K) when the effect of thermal acti-vation is negligible. For each crystal, we simulate indenta-tion on the (111), (110) and (100) surfaces, and quantifythe critical conditions of homogenous dislocation nucle-ation in the bulk perfect crystal. The results highlight thecentral role of hyperelasticity (nonlinear elasticity) andcrystallography in dislocation nucleation in small materialvolumes, a process requiring ultra-high stress that isachievable during nanoindentation. Our study also revealsthe deficiency of commonly used nucleation criterion suchas the critical resolved shear stress. With the rapid develop-ment in the experimental techniques of nanoindentation[6], we envision a direct comparison will soon becomepossible between the experiments (where a further improve-ment for quantitative control is needed) and atomistics-based quantification of critical conditions of dislocationnucleation as predicted in this paper.
2. Method
2.1. Interatomic potential finite element method
The key to the interatomic potential finite elementmethod (IPFEM) is the interatomic potential-based consti-tutive relation derived within the framework of hyperelas-ticity with the Cauchy–Born rule [10]. The basic premiseof this approach is that every point in a continuum corre-sponds to a large region of uniformly deformed lattice atthe atomic scale. It follows that the energy of a continuumpoint can be calculated by summing the energy of theunderlying lattice deformed according to the continuumdeformation gradient, Fij. Specifically, for a continuumpoint, all underlying atoms are identical, one may considerthe energy of one atom at the origin to be representative,and calculate the energy associated with this atom; theenergy density is the energy per atom divided by the atomicvolume. Within the framework of the embedded-atommethod (EAM) [11], and consider the crystal at nearlyzero-K temperature, the energy density W is given by
W ¼ 1
X0
XK
V ðrKÞ þ Uð�qÞ" #
; ð1Þ
where V(rK) is the pair potential, �q ¼P
KqðrKÞ is the ambi-ent electron density for the atom at the origin, and Uð�qÞ isthe energy required to embed this atom into the electrondensity. In Eq. (1), X0 is the atomic volume in a stress freefcc lattice, namely, X0 ¼ a3
0=4, where a0 is lattice constant;rK denotes the distance between the atom at the origin anda neighboring atom when the lattice is deformed, here, theindex K runs over all atoms within a cut-off radius Rc pre-scribed by the interatomic potential.
The Cauchy (true) stress can be obtained using the stan-dard relation between energy density and stress,
rij ¼1
detðF ijÞF imF jn
oWoEmn
: ð2Þ
In Eq. (2), the Green strain Eij is defined as Eij ¼12ðF kiF kj � dijÞ, where dij denotes the Kronecker delta; the
energy density W, as defined in Eq. (1) depends on Eij
through rK ¼ffiffiffiffiffiffiffiffiffiffiffiffiffiffiffiffiffiffiffiffiffiffiffiffiffiffiffiffiffiffiffiffiðdij þ 2EijÞxK
0ixK0j
q, where xK
0j is the coordinate
of a neighboring atom in the stress-free fcc lattice. Substi-tution of Eq. (1) into Eq. (2) leads to
rij ¼1
detðF ijÞX0
�X
K
1
2
oV ðrKÞor
þ oUð�qÞo�q
oqðrKÞor
� �xK
i xKj
rK: ð3Þ
Here xKj denotes the Cartesian coordinate of a neighboring
atom in the deformed lattice, and it can be calculated byxK
j ¼ F ijxK0j. Since the Cauchy stress in Eq. (3) involves lat-
tice sum and nonlinear functions of V(rK), Uð�qÞ and q(rK)[12,13], the effects of crystal anisotropy and nonlinear elas-ticity are incorporated automatically.
The tangent modulus, cijkl, can also be calculated fromthe interatomic potential, as detailed in [9],
cijkl ¼1
detðF ijÞX0
XK
1
2
oV 2ðrKÞor2
� 1
rK
oV ðrKÞor
� ��(
þ oUð�qÞo�q
o2qðrKÞor2
� 1
rK
oqðrKÞor
� ��xK
i xKj xK
k xKl
ðrKÞ2
þ o2Uð�qÞo�q2
XK
oqðrKÞor
xKi xK
j
rK
! XK
oqðrKÞor
xKk xK
l
rK
!):
ð4Þ
Here, the current and reference configurations are assumedto coincide. Because of the elastic softening of the hyper-elastic crystal, the prediction of dislocation nucleation(see Section 2.3) requires an update of the tangent moduluscijkl when deformation gradient Fij changes.
The above interatomic potential-based constitutivemodel can accurately describe the hyperelastic responseof a bulk crystal, whereas it is inadequate to model the elas-tic behavior of atomic layers near the crystal surface [14],where atoms are mis-coordinated compared to the perfectcrystal. However, since we will consider the indenter witha tip radius of 50 nm (an approximate size in experiments),the nucleation sites are located at about 10 nm below thecontact surface, so that the effect of mis-coordinated sur-face atoms are negligible. As such, this constitutive modelis sufficient to study nanoindentation-induced dislocationnucleation inside the bulk crystal, as verified by moleculardynamics simulations [9].
The interatomic interactions are modeled using theEAM potentials [11], which can better describe the many-body effects of metallic bonding compared to the two-bodypair potential such as Lennard–Jones potential. The EAMpotentials used in this study are developed by Mishin et al.[12,13], which have been validated by comparing withexperimental results (if available) and/or ab initio cal-culations. Table 1 compares the elastic constants of the
Table 1Elastic constants of stress-free single crystals of Cu, Ni and Al
c11 (GPa) c12 (GPa) c44 (GPa) b � 2c44
c11�c12
Cu Experiment 168.4 121.4 75.4 3.2Potential 169.9 122.6 76.2
Ni Experiment 247 147 125 2.5Potential 247 148 125
Al Experiment 114 61.9 31.6 1.2Potential 114 61.6 31.6
Predictions by the EAM potentials are compared with experimental data.b � 2c44/(c11 � c12) measures the degree of crystal anisotropy.
Fig. 1. Stress–strain curves for simple shear of single crystals of Al, Cu, Niin the Shockley partial direction of f111gh11�2i, showing the nonlinearelasticity and asymmetry of shear stress with respect to the sense ofshearing at large deformation.
3176 Y. Zhong, T. Zhu / Comput. Methods Appl. Mech. Engrg. 197 (2008) 3174–3181
stress-free crystals (Cu/Ni/Al) between experiments andpredictions by the potentials. It also lists the crystal-anisot-ropy parameter b � 2c44/(c11 � c12); for isotropic materials,b = 1.
We have implemented this interatomic potential-basedhyperelastic model for the fcc crystals of Cu, Al and Niin the finite element program ABAQUS/Explicit (2006)by writing user material subroutines. In the dynamic, expli-cit computational procedures of this program, as detailedin ABAQUS Theory Manual [15], the nonlinear responseis obtained incrementally, given the internal forces createdby the stresses in the elements, as well as the applied exter-nal forces at the start of an increment, time t. Finite ele-ment procedures solve for the acceleration at the start ofthe increment by solving the discretized local equationsof motion. The velocities at time t + Dt/2 and the displace-ments at time t + Dt are updated by a central differencetime-integration procedure. The deformation gradient Fij
for each integration point at time t + Dt is then calculatedbased on the updated displacement field. Given the calcu-lated deformation gradient, a constitutive equation subrou-tine, called VUMAT in ABAQUS/Explicit, is required inorder to determine the stress in the element at timet + Dt. In the implementation of stress calculation accord-ing to Eq. (3), each material point (integration point) isrepresented by an fcc lattice, which deforms according tothe local continuum deformation gradient Fij. That is, atthe beginning of the calculation (t = 0), a set of neighbor-ing atoms is created to represent the atomic environmentof the central atom at the origin, e.g., an atom in the firstneighboring shell should be located at (a0/2, a0/2, 0), anatom in the second neighboring shell is at (a0, 0, 0), etc.Here, the lattice spacing a0 is chosen such that the Cauchystress is zero at t = 0, and the number of included neigh-boring atoms is determined by the cut-off radius prescribedby interatomic potentials [12,13]. For each time increment,the neighboring atoms update their positions according tothe local deformation gradient Fij, which is generatedaccording to the imposed boundary conditions. Then theCauchy stress rij and tangent modulus cijkl are calculatedby substituting the deformed positions of neighboringatoms into Eqs. (3) and (4), respectively. Thus, materialproperties depend exclusively on the atomistic descriptionof the system.
2.2. Nonlinear elasticity and shear asymmetry at large strain
In this section, we highlight the important features ofthe interatomic potential-based constitutive model: nonlin-
ear elasticity and shear asymmetry at large strain. Consideran fcc crystal undergoing uniform simple shear in theShockley partial direction of f1 11gh11�2i. Fig. 1 showsthe shear stress–strain curves predicted by the EAM poten-tials. Evidently, the crystal at large shear exhibits nonlin-earity and asymmetry of shear stress with respect to thesense of shearing in the h11�2i direction. The former canbe attributed to the elastic softening at large strain, whereasthe latter arises because of the asymmetric packing ofatoms in the h11�2i direction [9]. The two effects criticallycontrol when, where and how a dislocation homogeneouslynucleates beneath the indenter, as detailed in Section 3.
2.3. Dislocation nucleation criterion
Homogenous dislocation nucleation in the bulk perfectcrystal can be triggered by the nonlinear elastic instabilityof crystal at large deformation. The onset of instability isassociated with the Hadamard condition of loss of positivedefiniteness of the matrix Qjk defined by
Qjk ¼ niðcijkl þ rjkdilÞnl ð5Þ
for any unit vector ni [16,17]. Here, the current and refer-ence configurations are assumed to coincide; rjk is the Cau-chy (true) stress and cijkl is the tangent (instantaneouselastic) modulus, both of which are calculated from theinteratomic potential, see Eqs. (3) and (4). For small defor-mations, Qjk is positive definite. When
detðQjkÞ ¼ 0; ð6Þ
Fig. 2. Finite element mesh for indentation simulation. The sphericalindenter is modeled as a frictionless, analytic rigid surface. The simulationcell is one half of the whole system considering the cubic symmetry of thefcc crystal.
Y. Zhong, T. Zhu / Comput. Methods Appl. Mech. Engrg. 197 (2008) 3174–3181 3177
loss of stability occurs, leading to dislocation nucleation.Correspondingly, the unit vector ni predicts the activatedslip plane, and the eigenvector gi associated with the matrixQjk predicts the slip direction at the onset of dislocationformation. By comparing with MD simulations, we havequantitatively verified the accuracy of this nucleation crite-rion in terms of the predictions of the critical indentationload, location of nucleation site and activated slip systems[9].
To appreciate the key difference between the nucleationcriterion of Eq. (6) with the commonly used one such as thecritical resolved shear stress (CRSS), we note that Qjk inEq. (6) contains both the tangent modulus cijkl and Cauchy(true) stress rjk. When a dislocation is about to nucleate(the corresponding shear strain is large), the magnitudesof cijkl and rjk become comparable due to elastic softeningof the hyperelastic crystal; the nucleation criterion of Eq.(6) states that when the decreasing cijkl is balanced withthe increasing rjk, the crystal becomes unstable, leadingto homogenous dislocation nucleation. Since the instabilitydoes not occur precisely when the tangent modulus van-ishes (equivalently, the RSS maximizes), the nucleation cri-terion based on the CRSS is not accurate. Moreover, theCRSS is not a material constant; it depends on other stresscomponents than just the shear. Thus, even an approxi-mate use of CRSS to predict nucleation would require acalibration for different stress (deformation) states, similarto the construction of a yield surface in stress space in theplasticity theory. In contrast, the nucleation criterion ofEq. (6) does not require calibration; nucleation occurs asa natural consequence of loss of positive definiteness ofthe matrix Qjk.
2.4. Simulation setup
Using the IPFEM, we have performed 3D simulationsof nanoindentation by a spherical indenter, and quantifiedthe critical states of dislocation nucleation. Predictions willbe given as to when and where the dislocation will nucleatewithin the crystal, and what slip mode the nucleated dislo-cation will take. More specifically, indentation is simulatedfor a spherical indenter pressed into the (111), (110) and(100) surfaces of single crystals of Al, Cu, Ni. The radiusof the indenter is 50 nm, the approximate tip size of a nom-inally sharp Berkovich indenter used in typical nanoinden-tation experiments. The spherical indenter is modeled as africtionless, analytic rigid surface. Since this research isfocused on dislocation nucleation inside the bulk crystal,the effects of indenter elasticity and contact adhesion areignored. However, those effects could play an importantrole if a dislocation nucleate directly from the contact sur-face [18,19]; a detailed study of surface nucleation isbeyond the scope of this work. We have previously per-formed extensive numerical testing to assess the influencesof geometry of simulation cell, imposed far-field boundaryconditions, element type, and node density by comparingwith the Hertzian solutions for the isotropic and aniso-
tropic, linear elastic material, as detailed in [9]. We foundfor a system with the in-plane size of 300 · 300 and depthof 600 nm, the effect of boundary constraint is sufficientlyminimized. To reduce the computational cost, we simulateone half of the whole system considering the cubic symme-try of crystal, as shown in Fig. 2. The boundary conditionsare imposed as follows: the displacement along the bottomof the mesh is constrained to be zero, while the displace-ments of lateral surfaces are unconstrained. The gradedmesh comprises 8-node linear brick elements, with typicalsize of elements near the indenter about 10 A. The totalnumber of elements is 519,332. Indenter is moved downin displacement control at a sufficiently low rate to mimicthe quasi-static loading condition, as calibrated by the ana-lytic solutions for indentation on a linear anisotropic elas-tic material [9].
3. Results and discussions
3.1. Indentation load–displacement response
Fig. 3a–c show the load–displacement (P–h) curves fornanoindentation on single crystals of Al, Cu and Ni,respectively. For each crystal, the P–h curves are calculatedfor three indentation orientations (111)/(0 11)/(0 01). Thedifferent P–h responses arise because of the elastic anisot-ropy of single crystals. For Al, the three P–h curves arevery close, consistent with the fact that Al is a nearly iso-tropic material (b = 1.2, see Table 1). As the elastic anisot-ropy increases, i.e., from b = 2.5 for Ni to b = 3.2 for Cu,the variation in the P–h responses also increases for differ-ent indentation orientations. These results are consistentwith the variation of indentation moduli given in Table 2,where the crystal is simplified as a linear, anisotropic andelastic material; such simplification renders the indentationmoduli analytically solvable, thus providing a quantitativereference to the numerical calculation for the hyperelastic
Fig. 3. Nanoindentation load–displacement curves for indentation on the (111), (110), (100) surfaces of single crystals of (a) Al, (b) Cu and (c) Ni. The(111) indentations are compared in (d) for the three crystals.
3178 Y. Zhong, T. Zhu / Comput. Methods Appl. Mech. Engrg. 197 (2008) 3174–3181
crystals. We note that the crystal beneath the nanoindentershould have undergone nonlinear elastic deformationbefore homogenous dislocation nucleation. But the effectof nonlinearity is not significant on the P–h response. This
Table 2Indentation moduli, E*, for single crystals of Al, Cu and Ni
E�ð1 1 1Þ ðGPaÞ E�ð1 0 0Þ ðGPaÞAl 88.9 87.1Cu 153 135Ni 254 228
They are calculated by numerical integration using the semi-analyticindentation solution, with the elastic constants predicted by the inter-atomic potentials, as listed in Table 1. Specifically, when a cubic crystaldeforms in the regime of linear anisotropic elasticity, the P–h response canbe derived as P ¼ 4
3 E�R1=2h3=2 for a spherical indenter (radius R) on a halfspace; for the (111) and (100) indentations, it can be proven that thecontact area is circular because of crystal symmetry, and the semi-analyticsolution is given by [20,21].
is because the P–h curve is not a particularly sensitive indi-cator on the nonlinear elastic deformation during nanoin-dentation, as it represents an average of the linear elasticresponse at the far field and the nonlinear elastic responseclose to indenter. However, the hyperelastic constitutivemodel, which is the basis of IPFEM simulations, is essen-tial to predict dislocation nucleation caused by the nonlin-ear elastic instability of crystals at large shear, as shown inSection 3.3.
In Fig. 3a–c, each P–h curve is terminated at an inden-tation depth (indicated by circle), when the onset of dislo-cation nucleation is first identified by the nucleationcriterion of Eq. (6). For each crystal, the critical load ofnucleation (Pc and hc) changes considerably for differentindentation orientations, e.g., hf1 1 1g
c : hf1 1 0gc : hf1 0 0g
c �5:04 nm : 3:85 nm : 1:93 nm � 2:6 : 2 : 1 for Cu. Thischange arises because of the effect of crystallography, asfirst shown in Wang et al. [22]. Specifically, consider a sim-ple situation of dislocation nucleation in the bulk singlecrystal under a uniaxial compressive stress r. In this case
Y. Zhong, T. Zhu / Comput. Methods Appl. Mech. Engrg. 197 (2008) 3174–3181 3179
a dislocation tends to nucleate on one of the f111gh11�2islip systems, where the resolved shear stress s = mr (mdenotes the Schmid factor) first exceeds the shear resistanceof nucleation in a perfect lattice. By considering the hardsphere packing of an fcc lattice and noting the effect ofshear asymmetry as shown in Fig. 1, one can readily calcu-late m and identify the slip system of nucleation; for differ-ent compression orientations, the ratio of the inverseSchmid factor is 1/m{1 1 1}: 1/m{1 1 0}: 1/m{1 0 0} = 3:2:1.One may assume the shear resistance of nucleation sc isthe same for each case, and then obtains rf1 1 1g
c :rf110g
c : rf1 0 0gc ¼ 3 : 2 : 1; here, in a first approximation we
ignore the influence of other stress components on sc.The ratio of rc for different compression orientations isqualitatively consistent with that of the nucleation loadhc for different indentation orientations, thereby showingthat the variation of hc is dominantly controlled by theeffect of crystallography. While the above simple analysisclarifies the controlling factor on hc, the IPFEM calcula-tions enable quantification of Pc and hc by solving the dis-tribution of nonuniform and nonlinear elastic deformationbeneath the indenter, as shown in Fig. 3.
In Fig. 3d, we compare the P–h curves for the (111)indentation of the three crystals. It is seen that Ni is muchstiffer than Cu and Al, consistent with the result that Ni hasa higher indentation modulus as shown in Table 2. In termsof the critical indentation displacements of nucleation, hc, itis interesting to note that although Cu and Al show verysimilar response for uniform simple shear (see Fig. 1), theirhc differ considerably; such difference arises because of crys-tal anisotropy, as well as the nonuniform deformationbeneath the indenter, as manifested in the different indenta-tion moduli (see Table 2).
Fig. 4. IPFEM predictions of nucleation sites by nanoindentation on the (100)nucleation sites; all the solid lines are in the h110i directions and the shaded tricritical moment of nucleation and for the respective activated slip plane. Thedet(Qjk), thus showing the nucleation sites. (For interpretation of the referencesof this article.)
3.2. Nucleation site and activated slip system
Fig. 4 shows the predicted nucleation sites from IPFEMcalculations, using Al as an example. As schematicallyshown in Fig. 4a, the nucleation site for the (100) indenta-tion is at the central loading axis. In contrast, it is off thecentral axis for the (110) and (111) indentations; the num-ber of equivalent sites, as well as their locations, is dictatedby crystal symmetry, see [9] for example. In Fig. 4b, weshow the contours of det(Qjk) at the respective criticalmoment of nucleation and for the respective activated slipsystem. In each case, the gray element (highlighted with redcircles) indicates the nucleation site directly visible on thesurface of the simulation cell. Because of the high symme-try of indentation orientations, there are multiple equiva-lent slip systems at each site; the slip system firstactivated in experiment or MD simulation would be ran-domly selected by thermal fluctuations. Our predictionsby IPFEM, which accurately incorporate the effects of elas-tic softening and crystal anisotropy, have been qualitativelyverified by MD simulations [22]; but they are at variancewith predictions based on the linear elastic analysis [23]and/or using the stress-based nucleation criterion such asthe maximum equivalent shear stress or CRSS [24].
3.3. Critical resolved shear stress
We calculate the critical resolved shear stress (CRSS), sc,at the onset of nucleation, and show the CRSS is not anaccurate nucleation criterion. Fig. 5 shows the indentationdisplacement versus RSS curves. The RSS, s, is calculatedat the critical nucleation site and for the activated slip sys-tem, according to s = rijnigj, where the current slip-plane
, (110) and (111) surfaces of single crystal Al. (a) Schematics of location ofangles represent the {111} plane. (b) Contours of det(Qjk) at the respective
gray element (highlighted with red circles) has a small negative value ofto colour in this figure legend, the reader is referred to see the web version
Fig. 5. Nanoindentation displacement versus resolved shear stress at thecritical nucleation site and for the activated slip system for single crystalsof Al, Cu and Ni.
Table 3The critical resolved shear stress (CRSS) of dislocation nucleation at therespective nucleation site for nanoindentation of single crystals Al, Cu andNi with three indentation orientations
(111) (110) (100)
sc–Cu (GPa) 3.2 3.0 2.3sc–Al (GPa) 3.8 4.0 3.1sc–Ni (GPa) 8.2 8.0 4.5
3180 Y. Zhong, T. Zhu / Comput. Methods Appl. Mech. Engrg. 197 (2008) 3174–3181
normal, ni, and slip direction, gi, are related to those in theunformed crystal, n0j and g0j, by ni ¼ n0jF �1
ji and gi = Fijg0j,respectively. In Fig. 5, circle represents the CRSS, sc, when
the nucleation criterion is first satisfied in IPFEM calcula-tions. The respective sc is listed in Table 3 for the threecrystals and three indentation orientations. Importantly,sc is not a constant for each crystal, and it depends onthe indentation orientation. Fig. 5 also shows that sc isclose to, but not right at the maximum of RSS. This isdue to the elastic-softening effect associated with the hyper-elastic crystals; namely, according to the physically basednucleation criterion of Eq. (5), the nucleation occurs whenthe tangent modulus cijkl is balanced with the Cauchy stressrij, rather than when cijkl vanishes or equivalently the RSSmaximizes. Hence, these results clearly demonstrate thatthe CRSS is NOT an accurate nucleation criterion; anapproximate use of CRSS needs a calibration by combin-ing experiments and IPFEM calculations.
Finally, we note that Fig. 5c reveals a numerical artifactof the RSS response for Ni under the (110) indentation,i.e., there is an abrupt change of the slope at low loads.Considering the overall reliable performance of the EAMpotentials, which have been extensively calibrated by com-paring with experimental or ab inito data [12,13], webelieve such a small artifact should not affect the overallreliability of the results reported in this study.
4. Summary and conclusions
We have simulated nanoindentation and predicted dislo-cation nucleation in fcc single crystals of Al, Cu and Ni.Simulations are performed using the interatomic potentialfinite element method, which is a computationally efficientapproach that facilitates the study at length scales largecompared to atomic dimensions, while remaining faithfulto the nonlinear interatomic interactions. We considerhomogenous dislocation nucleation triggered by the non-linear elastic instability of crystal at large strain and nearlyzero-K temperature. The results show that the criticalresolved shear stress of nucleation is at the GPa-level, closeto the theoretical limit of perfect crystals. However, thecritical conditions of dislocation nucleation, including theindentation load of nucleation, location of nucleation site,nucleation stress and activated slip systems, sensitivelydepend on the indentation orientation. But these condi-tions are consistent for different fcc crystals. Our studyhighlights the critical role of hyperelasticity (nonlinear elas-ticity) and crystallography in homogenous dislocationnucleation, and reveals the deficiency of commonly usednucleation criterion such as the critical resolved shearstress.
Y. Zhong, T. Zhu / Comput. Methods Appl. Mech. Engrg. 197 (2008) 3174–3181 3181
We conclude by commenting that for a complete under-standing of defect formation by nanoindentation, one needsto take into account the influences of finite temperature [25],structural heterogeneities (e.g., surface step [18]), pre-exist-ing dislocations [26], as well as the effect of homogenouslynucleated dislocations on subsequent nucleation [7,27].Recent development in the activation analysis of thermallyactivated dislocation nucleation at the interface [28], surface[29], and pre-existing defect [30,31], provides a viableapproach to address these issues. With the results from thisstudy as input (e.g., critical loads, nucleation sites and acti-vated slip systems), we envision the activation analysis ofnucleation during nanoindentation will enable a quantita-tive connection between experiments and modeling.
Acknowledgements
This work is supported by NSF Grant CMMI-0653769and AFOSR/MURI Grant F49620-02-1-0382. We thankKe Lu and Ju Li for stimulating discussions.
References
[1] T.F. Page, W.C. Oliver, C.J. McHargue, The deformation-behaviorof ceramic crystals subjected to very low load (nano)indentations, J.Mater. Res. 7 (2) (1992) 450–473.
[2] W.W. Gerberich, J.C. Nelson, E.T. Lilleodden, P. Anderson, J.T.Wyrobek, Indentation induced dislocation nucleation: the initial yieldpoint, Acta Mater. 44 (1996) 3585–3598.
[3] A. Gouldstone, H.J. Koh, K.Y. Zeng, A.E. Giannakopoulos, S.Suresh, Discrete and continuous deformation during nanoindentationof thin films, Acta Mater. 48 (2000) 2277–2295.
[4] W. Wang, K. Lu, Nanoindentation study on elastic and plasticanisotropies of Cu single crystals, Philos. Mag. 86 (2006) 5309–5320.
[5] A.M. Minor, S.A.S. Asif, Z.W. Shan, E.A. Stach, E. Cyrankowski, T.J.Wyrobek, O.L. Warren, A new view of the onset of plasticity during thenanoindentation of aluminium, Nat. Mater. 5 (2006) 697–702.
[6] A. Gouldstone, N. Chollacoop, M. Dao, J. Li, A.M. Minor, Y.L.Shen, Overview No. 142: indentation across size scales and disci-plines: Recent developments in experimentation and modeling, ActaMater. 55 (2007) 4015–4039.
[7] J. Li, K.J. Van Vliet, T. Zhu, S. Yip, S. Suresh, Atomistic mechanismsgoverning elastic limit and incipient plasticity in crystals, Nature 418(6895) (2002) 307–310.
[8] K.J. Van Vliet, J. Li, T. Zhu, S. Yip, S. Suresh, Quantifying the earlystages of plasticity through nanoscale experiments and simulations,Phys. Rev. B 67 (2003) 104105.
[9] T. Zhu, J. Li, K.J. Van Vliet, S. Ogata, S. Yip, S. Suresh, Predictivemodeling of nanoindentation-induced homogeneous dislocationnucleation in copper, J. Mech. Phys. Solid 52 (2004) 691–724.
[10] J.L. Ericksen, The Cauchy and Born hypotheses for crystals, in: M.E.Gurtin (Ed.), Phase Transformations and Material Instabilities inSolids, Academic Press, New York, 1984, pp. 61–78.
[11] M.S. Daw, M.I. Baskes, Embedded-atom method – derivation andapplication to impurities, surfaces, and other defects in metals, Phys.Rev. B 29 (1984) 6443–6453.
[12] Y. Mishin, D. Farkas, M.J. Mehl, D.A. Papaconstantopoulos,Interatomic potentials for monoatomic metals from experimentaldata and ab initio calculations, Phys. Rev. B 59 (5) (1999) 3393–3407.
[13] Y. Mishin, M.J. Mehl, D.A. Papaconstantopoulos, A.F. Voter, J.D.Kress, Structural stability and lattice defects in copper: ab initio,tight-binding, and embedded-atom calculations, Phys. Rev. B 63 (22)(2001) 224106.
[14] H.S. Park, P.A. Klein, G.J. Wagner, A surface Cauchy–Born modelfor nanoscale materials, Int. J. Numer. Method Engrg. 68 (2006)1072–1095.
[15] ABAQUS, Theory Manual. Hibbitt, Karlsson and Sorensen Inc.,Pawtucket, R.I., 2006.
[16] R. Hill, Acceleration Waves in Solids, J. Mech. Phys. Solid 10 (1962)1–16.
[17] J.R. Rice, The localization of plastic deformation, in: W.T. Koiter(Ed.), Proceedings of the 14th International Congress on Theoreticaland Applied Mechanics, North-Holland Publishing Co., Amsterdam,1976, pp. 207–220.
[18] J.A. Zimmerman, C.L. Kelchner, P.A. Klein, J.C. Hamilton, S.M.Foiles, Surface step effects on nanoindentation, Phys. Rev. Lett. 8716(2001) 165507.
[19] H.H. Yu, P. Shrotriya, Y.F. Gao, K.S. Kim, Micro-plasticity ofsurface steps under adhesive contact: Part I – Surface yieldingcontrolled by single-dislocation nucleation, J. Mech. Phys. Solid 55(2007) 489–516.
[20] J.G. Swadener, G.M. Pharr, Indentation of elastically anisotropichalf-spaces by cones and parabolae of revolution, Philos. Mag. A –Phys. Conden. Mat. Struct. Defect Mech. Proper. 81 (2001) 447–466.
[21] Y.F. Gao, G.M. Pharr, Multidimensional contact moduli of elasti-cally anisotropic solids, Scripta Mater. 57 (2007) 13–16.
[22] W. Wang, Y. Zhong, T. Zhu, K. Lu, Quantifying the onset ofplasticity during nanoindentation: experiment and modeling (inpreparation).
[23] H. Bei, E.P. George, J.L. Hay, G.M. Pharr, Influence of indenter tipgeometry on elastic deformation during nanoindentation, Phys. Rev.Lett. 95 (2005) 045501.
[24] T. Tsuru, Y. Shibutani, Anisotropic effects in elastic and incipientplastic deformation under (001), (110), and (111) nanoindentation ofAl and Cu, Phys. Rev. B 75 (2007) 035415.
[25] C.A. Schuh, J.K. Mason, A.C. Lund, Quantitative insight intodislocation nucleation from high-temperature nanoindentation exper-iments, Nat. Mater. 4 (2005) 617–621.
[26] A.H.W. Ngan, P.C. Wo, Delayed plasticity in nanoindentation ofannealed crystals, Philos. Mag. 86 (2006) 1287–1304.
[27] H.Y. Liang, C.H. Woo, H.C. Huang, A.H.W. Ngan, T.X. Yu,Crystalline plasticity on copper (001), (110), and (111) surfacesduring nanoindentation, Cmes-Comput. Model. Engrg. Sci. 6 (2004)105–114.
[28] T. Zhu, J. Li, A. Samanta, H.G. Kim, S. Suresh, Interfacial plasticitygoverns strain rate sensitivity and ductility in nanostructured metals,Proc. Natl. Acad. Sci. USA 104 (2007) 3031–3036.
[29] T. Zhu, J. Li, A. Samanta, A. Leach, K. Gall, Temperature andstrain-rate dependence of surface dislocation nucleation, Phys. Rev.Lett., in press.
[30] T. Zhu, J. Li, S. Yip, Atomistic study of dislocation loop emissionfrom a crack tip, Phys. Rev. Lett. 93 (2004) 025503.
[31] T. Zhu, J. Li, S. Yip, Atomistic configurations and energetics of crackextension in silicon, Phys. Rev. Lett. 93 (2004) 205504.