WELDING PROCEDURE SPECIFICATION (WPS) Yes …
Transcript of WELDING PROCEDURE SPECIFICATION (WPS) Yes …
![Page 1: WELDING PROCEDURE SPECIFICATION (WPS) Yes …](https://reader030.fdocuments.in/reader030/viewer/2022012711/61aaf535f08ebd6b0e16ca93/html5/thumbnails/1.jpg)
ANNEX N AWS D1.1/D1.1M:2008
348
WELDING PROCEDURE SPECIFICATION (WPS) Yes PREQUALIFIED __________ QUALIFIED BY TESTING __________
or PROCEDURE QUALIFICATION RECORDS (PQR) Yes
WELDING PROCEDURE
Identification # _________________________________Revision _______ Date__________ By ____________
Company Name _______________________________ Authorized by __________________ Date __________Welding Process(es) ____________________________ Type—Manual Semiautomatic Supporting PQR No.(s) __________________________ Machine Automatic
JOINT DESIGN USED POSITIONType: Position of Groove:______________ Fillet: __________Single Double Weld Vertical Progression: Up Down Backing: Yes No Backing: Backing Material: ELECTRICAL CHARACTERISTICSRoot Opening ______ Root Face Dimension ________ ______________________Groove Angle: ___________ Radius (J–U) _________ Transfer Mode (GMAW) Short-Circuiting Back Gouging: Yes No Method _______ Globular Spray
Current: AC DCEP DCEN Pulsed BASE METALS Power Source: CC CV Material Spec. _________________________________ Other ________________________________________Type or Grade _________________________________ Tungsten Electrode (GTAW)Thickness: Groove ____________ Fillet __________ Size: ______________Diameter (Pipe)________________________________ Type: ______________
FILLER METALS TECHNIQUEAWS Specification______________________________ Stringer or Weave Bead: _________________________AWS Classification _____________________________ Multi-pass or Single Pass (per side)_________________
Number of Electrodes ___________________________Electrode Spacing Longitudinal ____________
SHIELDING Lateral_________________Flux ___________________ Gas _________________ Angle _________________
Composition __________ Contact Tube to Work Distance ____________________Electrode-Flux (Class)_____ Flow Rate ____________ Peening ____________________________________________________________ Gas Cup Size _________ Interpass Cleaning: _____________________________
PREHEAT POSTWELD HEAT TREATMENTPreheat Temp., Min. ____________________________ Temp. ________________________________________Interpass Temp., Min. ___________ Max. _________ Time _________________________________________
Pass or Weld
Layer(s) Process
Filler Metals Current
VoltsTravelSpeed Joint DetailsClass Diam.
Type &Polarity
Amps or Wire Feed Speed
Form N-1 (Front)
![Page 2: WELDING PROCEDURE SPECIFICATION (WPS) Yes …](https://reader030.fdocuments.in/reader030/viewer/2022012711/61aaf535f08ebd6b0e16ca93/html5/thumbnails/2.jpg)
ANNEX N AWS D1.1/D1.1M:2008
352
Procedure Qualification Record (PQR) # __________Test Results
VISUAL INSPECTIONAppearance___________________________________ Radiographic-ultrasonic examinationUndercut _____________________________________ RT report no.: __________ Result ________________Piping porosity ________________________________ UT report no.: ___________ Result ________________Convexity_____________________________________ FILLET WELD TEST RESULTSTest date _____________________________________ Minimum size multiple pass Maximum size single passWitnessed by__________________________________ Macroetch Macroetch
1. _______ 3. ________ 1. ________ 3. ________2. _______ 2. ________
Other Tests All-weld-metal tension test
Tensile strength, psi _____________________________Yield point/strength, psi __________________________Elongation in 2 in, % ____________________________
Laboratory test no. _________________________
Welder’s name ________________________________ Clock no. ______________ Stamp no._____________
Tests conducted by _________________________________________________________ Laboratory
Test number ___________________________________
Per __________________________________________
We, the undersigned, certify that the statements in this record are correct and that the test welds were prepared, welded, andtested in conformance with the requirements of Clause 4 of AWS D1.1/D1.1M, (__________) Structural Welding Code—Steel.
(year)
Signed _______________________________________Manufacturer or Contractor
By ___________________________________________
Title _________________________________________
Date _________________________________________
Form N-1 (Back)
TENSILE TEST
SpecimenNo.
Width Thickness AreaUltimate Tensile
Load, lbUltimate UnitStress, psi
Character of Failure and Location
GUIDED BEND TEST
SpecimenNo.
Type of Bend Result Remarks
![Page 3: WELDING PROCEDURE SPECIFICATION (WPS) Yes …](https://reader030.fdocuments.in/reader030/viewer/2022012711/61aaf535f08ebd6b0e16ca93/html5/thumbnails/3.jpg)
SUBCONTRACTOR: CONTECH ENGINEERING Co. LLC I WELDING PROCEDURE SPECIFICATION No. WPS/1435/02 Rev-01
WELDING PROCEDURE SPECIFICATION Scope: GENERAL WELDING & AND REPAIR OF PROCEDURE QUALIFICATION RECORD No(s).
APPLICABLE FOR SMAW(ROOT)+ BUTT JOINTS & FILLET WELDS USING OBI 990650/09FCAW(OTHERS) PROCESS
SMAW + FCAW PROCESS IN ALL POSITIONSRT/24100/04, M2973·1 PCOMPLIANCE TO SPECIFICATIONS OF
ADCOP 30.99.75.1603, 30.99.75.1611. M2973·1M1JEBEL All YARD.
Project: FABRICATION & INSTALLATION OF STEEL BRIDGES CE Job No. J 1435ADCOP-ABUDHABI CRUDE OIL PIPELINE PROJECT-HABSHAN TO FUJAIRAH
QUALIFICATION IN ACCORDANCE WITH AWS 01.1WELDING PROCESS : SMAW ROOT) + FCAW TYPE : SMAW+FCAWBASE METAL : BS EN 10210 - S355 J2H or Equivalent QUALIFIED THICKNESS RANGE : 4.8mm. TO Unlimited.QUALIFIED COMPONENT CATEGORY: STRUCTURAL STEEL POSITION : 6G UPHILL - BUTT JOINTSCARBON EQUIVALENT : Max 0.45 QUALIFIED DIAMETER RANGE : 100mm. & ABOVE
....•.... TECHNIQUE:~ CloP MAXIMUM WELD : 15mm.
t ~
BEAD WIDTHPREPARATION METHOD FLAME CUT & GROUND BY 2mm MINIMUMumm·DLJ TACK WELD : SAME AS WITH ROOT PASS
:t:l.5mm. -L-TACK LENGTH : 50mm. MINIMUM----il .OTTREATMENT OF SECOND SIDE : N/A.1.4mm.
!u••••. GOUGING METHOD : N/A.INTERPASS CLEANINGALL SCALE OR SLAG SHALL BE REMOVED BEFORE DEPOSITING THE NEXT PRE-HEAT TEMPERATURE TABLE:SUCCESSIVE BEAD.DEFECTS ANY UNACCEPTABLE DISCONTINUITY THAT APPEARS ON THE SURFACE ON THICKNESS (mm.)
MINIMUM PRE-HEATANY BEAD SHALL BE REMOVED BY GRINDING BEFORE DEPOSITING THE NEXT TEMPERATURE °CSUCCESSIVE BEAD
TYPE OF EDGE PREPARATION: AS ALLOWED BY THE CODE· BACK GRINDING IUPTO 19 21
19 < t < 38.1 66GOUGING IN DOUBLE SIDE GROOVE WELDING.OTHERS: ALSO QUALIFIES PJP WELDS AND FILLET WELDS OF ALL THICKNESS. 38.1 < t s 63.5 107
OVER 63.5 150PRE-HEAT METHOD OXY FUEL GAS HEATERS IF BELOW 21·C.MAXIMUM INTERPASS TEMP.: 260·CPEENING : NlA.
WELDING ELECTRODE(S) FLUX OR GAS WELDING STICK Heatill WELDING FLOW WFS0 RUN No. POSITION I GAS AMPS VOLTS SPEED LENGTH Inputv; PROCESS DIRECTION TRADE SHIELD RATE mm.lmln (mm.) MlMn
KJ/mmSIZE NAME POLARITY Litlmm.
1 ROOT SMAW ALL UPHILL 2.5 ELGA DCSP N/A N/A 65 ·81 19 - 22 46-60 N/A N/A 1.24P47P
HYUNDAI1 HOT FCAW ALL UPHILL 1.2 SF·71 DCRP CO2 20·28 151· 206 22-25 109-131 18·25 ... 283
1 FILL FCAW ALL UPHILL 1.2 HYUNDAI DCRP CO2 20·28 142·202 22 - 25 118·186 18·25 2.57SF·71...
1 CAP FCAW ALL UPHILL 1.2 HYUNDAI DCRP CO2 20·28 147 ·197 20-22 206·227 18·25 126SF·71_.
POST WELD TREATMENT FILLER METAL
WELD METAL No. 1 OthersHEATING RATE N/A.
F. No. 4 6
SPECIFICATION No.(SFA) 5.1 5.20SOAK TEMP. C· N/A.
AWS CLASSIFICATION E7016 A5·20 E71T·1
SOAK TIME N/A. TRADE NAME (ELECTRODE) ELGA Or Equivalent HYUNDAI SF·71 Or Equivalent
COOLING RATE N/A. TRADE NAME (FLUX) N/A N/A
WITHDRAWAL N/A. DIAMETER (mm.) 2.5 1.2
TEMPERATURE C· N/A. NOTES: Prior to Capping, the interpass temperature shall be between the minimum preheat temperature (Refer toPreheat table above) and the maximum internass temperature.
CONSUMABLE CONTROL· El016 I BAKING AROUND 350·C 2 Hrs. Min. I HOLDING TEMP. : 120·C Mn. I QUIVER TEMP. (SMAW) : Min 65·C
PREPARED By QA APPROVED BY
Company ~ONTECH ~CHEC CPECC TPI IPIClILF
Siqnature Pt&;~DPrint Name .~-Date 15.06.2OW
![Page 4: WELDING PROCEDURE SPECIFICATION (WPS) Yes …](https://reader030.fdocuments.in/reader030/viewer/2022012711/61aaf535f08ebd6b0e16ca93/html5/thumbnails/4.jpg)
SUBCONTRACTOR: CONTECH ENGINEERING Co. LLC I WELDING PROCEDURE SPECIFICATION No. WPS/CE/02 Rev·01
WELDING PROCEDURE SPECIFICATION Scope: GENERAL WELDING & AND REPAIR OF PROCEDURE QUALIFICATION RECORD No(s).
APPLICABLE FOR SMAW(ROOT)+ Bun JOINTS & FILLET WELDS USING OBI 990650/09SMAW + FCAW PROCESS IN ALL POSITIONS
FCAW(OTHERS) PROCESS COMPLIANCE TO SPECIFICATIONS OF RT/241 00/04, M2973·1 PADCOP 30.99.75.1603.30.99.75.1611. M2973·1M1
JEBEL All YARD.QUALIFICATION IN ACCORDANCE WITH AWS D1.1
WELDING PROCESS : SMAW ROOT) + FCAW TYPE : SMAW+FCAWBASE METAL : 8S EN 10210· S355 J2H or Equivalent QUALIFIED THICKNESS RANGE : 4.&nm. TO Unlimited.QUALIFIED COMPONENT CATEGORY: STRUCTURAL STEEL POSITION : 6G UPHILL . BUTT JOINTSCARBON EQUIVALENT : Max 0.45 QUALIFIED DIAMETER RANGE : 100mm. & ABOVE
50"+10'".. TECHNIQUE:-:>: <»
i "~
MAXIMUM WELD : 15mm.BEAD WIDTHPREPARATION METHOD : FLAME CUT & GROUND BY 2mm. MINIMUMumm·DLJ TACK WELD · SAME AS WITH ROOT PASSiUhnm. .L,
OOT TACK LENGTH · SOmm. MINIMUM-----;1TREATMENT OF SECOND SIDE · NlA.3.4IIIm.
tu,. •. GOUGING METHOD : N/A.INTERPASS CLEM~INGALL SCALE OR SLAG SHALL BE REMOVED BEFORE DEPOSITING THE NEXT PRE·HEAT TEMPERATURE TABLE:SUCCESSIVE BEAD
THICKNESS (mm.)MINIMUM PRE·HEAT
DEFECTS ANY UNACCEPTABLE DISCONTINUITY THAT APPEARS ON THE SURFACE ON TEMPERATURE °CANY BEAD SHALL BE REMOVED BY GRINDING BEFORE DEPOSITING THE NEXTSUCCESSIVE BEAD. UPTO 19 21
TYPE OF EDGE PREPARATION AS ALLOWED BY THE CODE· BACK GRINDING / 19 < t s 38.1 66
GOUGING IN DOUBLE SIDE GROOVE WELDING. 38.1 < t s 63.5 107OVER 63.5 150
OTHERS: ALSO QUALIFIES PJP WELDS AND FILLET WELDS OF ALL THICKNESS. PRE·HEAT METHOD OXY FUEL GAS HEATERS IF BELOW 21·C.MAXIMUM INTERPASS TEMP.: 260·CPEENING : NlA.
WELDING aECTRODE(S) FLUX OR GAS WaDING STICK HeatUJ WELDING FLOW WFS0 RUN No. POSITION I GAS AMPS VOLTS SPEED LENGTH Inputin PROCESS DIRECTION TRADE SHIELD RATE mm.lmin. (mm.) MlMin. KJ!mm.SIZE NAME POLARITY Lit.lmm.
1 ROOT SMAW ALL UPHILL 2.5 aGA DCSP NlA NlA 65·81 19-22 46-60 N/A. N/A 124P47PHYUNDAI
1 HOT FCAW ALL UPHILL 1.2 SF-71 DCRP CO2 20 - 28 151 - 206 22-25 109 -131 18 - 25 --- 283
1 FILL FCAW ALL UPHILL 1.2 HYUNDAI DCRP CO2 20- 28 142 - 202 22 - 25 118 -186 18 - 25 2.57SF-71 ---
I CAP FCAW ALL UPHILL 1.2 HYUNDAI DCRP CO2 20- 28 147 - 197 20-22 206 - 227 18 - 25 1.26SF-71 ---
POST WELD TREATMENT FILLER METAL
WELD METAL No. 1 OthersHEATING RATE N/A
F No. 4 6
SPECIFICATION No.(SFA) 5.1 5.20SOAK TEMP. C· N/A.
AWS CLASSIFICATION E7016 A5-20 E71T·1
SOAK TIME N/A TRADE NAME (ELECTRODE) ELGA Or Equivalent HYUNDAI SF-71 Or Equivalent
COOLING RATE N/A. TRADE NAME (FLUX) N/A N/A
WITHDRAWAL N/A. DIAMETER (rnm.) 2.5 1.2
TEMPERATURE C· N/A.NOTES: Prior to Capping. the interpass temperature shall be between the minimum preheat temperature (Refer to
Preheat table above) and the maximum interpass temperature.
CONSUMABLE CONTROL. E7016 I BAKING AROUND 350·C 2 Hrs. Min. I HOLDING TEMP. : 120·C Mn. I QUIVER TEMP. (SMAW) : Min 65·C
PREPARED By QA APPROVED BY
Company CONTECH ENGINEERING Co. LLC ~I~~.....••'- M
. .~tM~L1oyd's egister EMEA-.Signature \:..'7 ' ?- I" ~ I 1
EDS ~-t\'\,,\L_ •••.. lovn,
Print Name ~2 ~'I~~~S~o f{eg{sferANBARASAN.P n"h" r
Date15·06·2010
![Page 5: WELDING PROCEDURE SPECIFICATION (WPS) Yes …](https://reader030.fdocuments.in/reader030/viewer/2022012711/61aaf535f08ebd6b0e16ca93/html5/thumbnails/5.jpg)
WELDING PROCEDUREQUALIFICATION RECORD (PQR)
Page 1 of 2
nt;./os/qqDate of issue
2166
107150
LROffice DUBAIPQRcertificatenumber
OBI 9900650/09IQualification:Codes/Standards
AWS Dl.lp wps. number and revision Date ofwelding Manufacturer's name and address
WPS/FCAW/99/01 26/04/99 CONTECH Engg. Co. LLCf-T-es-t-p-la-ce-/-loc-a-tio-n-s"'h;"op::'/-site-~-~----..L------~-~----------j Pos t Box - 5750
Con tech Workshop/ Jebel Ali / Dubai Dubaif-R-AN--G-E-O-F-AP-P-R-O-V-AL---------------------------j Uni ted Arab Emirates.Weldingprocess(es)SHAW (Root) + FCAW
Gas/flux100% C02 - FCAW
Progression (up/down)Uphill
Singlepass/multipass
MultipassJoint type(s)Single V - CJP
Plate thicknessrange
4.8mm. To Unlimited
Parent metal group(s)AWS Group I & IIPipe outside diameter range
100mm. & OverFillermetal type/ designation Heat treatment
F No.4 SFA5.1;FNo.6SFA5.~0 Not Applicable
50' I to"-6'.r<.
O.5mm·DI±O.5mm. -L "-------..I
Type of welding currentRoot-DCSP Others - DCRP
Weldingpositions6G
WELDANDFILLERMETALDETAILS ----111-1 ---3.4mm.±t.5mm.Parent Materials D2l9 1
Pipe - s355 J2H l?~7 x 6GWeldingprocess Joint type Beadsequencedetail (sketchto includeweld
Root-SHAW Others - FCAW Single V Groove - CJP metalthic.knessand back gougingwheref-F-ill-e=-r.:..ma-=te-rial-=·::....::.:=---...:~=---...:=-==---...::....::....--=---...:--+-S-hie-l-din~·~g-ga-s/-fl-u-x-flo-w-ra-te----------l applicable)
E7016 & E71T-l 20-28 Lits./mm.
Test pieceposition
CAP
\ ~~.::i /~ ~~
FlU ~ HOT PASS~n._~
Make/ type/ diameterELGA P47P & Hyundai SF71
Gas composition100% C02 - FCAW -,
Flux typeNot Applicable
Composition
Other information
Macro Examination also qualifies for PartialPenetration Joints.Fillet Unlimitted~---------------------------------------------------___!qpto 19Preheat and interpass temperature (method) and controlMaximum interpass Temp. 2600 C. 19~t~38.138.~~63.5Postweldheat treatment temperature (method) and control Over 63.5Not ApplicablePROCEDUREDETAIL
RUN PROCESS SIZE OF FILLER MATERIALNUMBER
1Root SMAW 2.5rrm.- E7016
2Hot FCAW 1.2rrm.- E71-Tl
Fill FCAW 1.2rrm.- E71-Tl
cap FCAW 1.2rrm.- E71-Tl
fll-tll°d«1e:;s mn. (t) Min. '.D:np~
1.829
CURRENT VOLTAGE ACjDC WlREFEED/ HEAT INPUTA V POLARITY TRAVEL SPEED kJ/mm
65-81 19-22 DCSP 46-60 1.235
151-172 22-25 DCRP 91-109
148-168 22-25 DCRP 118-186
.•.47-164 20-22 DCRP ~06-227
1.007
0.777
Date Welder'SnameMr. ANWAR KHAN05/05/99
·Manufacturer's PreliminaryWeldingProcedure Specification
WPQcertificatenumberDBI 9900650/15
FORM 5209 (ffij98) SHEET 1 OF 2 Lloyd'sRegisterofShipping, registered office:71FenchurchStreet, London EC3M4BS
THIS DOCUMENT IS SUBJECT TO THE TERMS AND CONDITIONS OVERLEAF
![Page 6: WELDING PROCEDURE SPECIFICATION (WPS) Yes …](https://reader030.fdocuments.in/reader030/viewer/2022012711/61aaf535f08ebd6b0e16ca93/html5/thumbnails/6.jpg)
Page 2 of 2WELDING PROCEDUREQUALIFICATION RECORD (PQR)- CONTINUED
LROffice
Dateofissue 05/05/99
PQRcertificatenumberOBI 9900650/09
TESTRESULTS Report No. : RT/24l00)f04NON-DESTRUCTIVE EXAMINATION (STATE 'ACCEPTABLE', 'UNACCEPTABLE' OR 'NONE')V,i$uaL. f IMagneticparticle Liquidpenetrant I Radioqraphl'.,at:.1S actory i lSatlstactory
I Ultrasonics
TEST
DESTRUCTIVE TESTS Report No. M2973-1p
Units
TENSILE YIELD
Transverse tensile
All-weld tensile
BEND TESTS
ORIENTATION
~t/ f,&/ side
~t/f~/side
l)e6t/ f~/ side
R)XS't/f~/ side
Longitudinal
IMPACT TESTS
RUN NUMBER
Requirement
Size10 Xl<h65
/Type Charpy,...
VNotchRetest
HARDNESS SURVEYType
VICKER
Parent Material
H.A.Z.
Weld
FORMER DIAMETER
38mm - 1800
38mm - 18d'
38mm - 180~
% REDUCTION OFAREA
% ELONGATION FRACTURE TEST
1.
FILLET WELD FRACTURE (RESULTS)
RESULTS
Satisfactory 2.
Satisfactory 3.
Satisfactory Macroexamination
NOTCH LOCATION/ TEMP VALUES (J) AVERAGE REMARKSORIENTATION ·C 1 2 3 (J)
WCL -20°c 48 98 94 80 Satisfactory
HAZ f-2d'c 172 194 120 162 Satisfactorv
I LoadHV 10
HARDNESS RANGE
157 - 176
202 - 294
207 - 268
Locationofhardnessmeasurements(sketch)
Satisfactory
Report No: M2973 - IMI
Additionaltest(s)andresult(s),egochemicalanalysis,microexamination,ferritemeasurement
~~ ~t~~ foregoing statements are correct and the test welds were prepared, welded and tested in accordance with the specified Codes!U9T ~andards ."
~q'~ ~c§!FORM 5209 (00/98) SHE~ 40 11 ~ egisterofShipping,registeredoffice:71 FenchurchStreet,LondonEC3M4BS
THIS DOCUMENT IS SUBJECT TO THE TERMS AND CONDITIONS OVERLEAF
![Page 7: WELDING PROCEDURE SPECIFICATION (WPS) Yes …](https://reader030.fdocuments.in/reader030/viewer/2022012711/61aaf535f08ebd6b0e16ca93/html5/thumbnails/7.jpg)
•___~L· .d\ V')~)".4. ~u J.-
~mitates :Jndusttial J!.a6otatotl{Oilfield, Marine & tndustriet Consultants Certificate No 943807
RADIOGRAPHIC REPORT RT/24100/04
Client:
Contech Engineering Co. LLC
P.O. Box - 5750
Dubai. U.A.E
ElL Job # 24100
Order Number Fax dtd. 28/04/99
Date Tested Apr. 29. 1999 i
Test Code ASME Sec. V
Acceptance Criteria AWSD1.1
Tested By 110
Operating Procedure OPN-001Attention: Mr. Subramanian
ProjectfVessel: Radiography on 8" dia. PQR pipe joints
Drawing No. Nil WPSjFCAWj99
PARAMETERS
Material Carbon steel
FilmThickness 8" dia. Sch.XS
Exposure Time 28 Ci. mts.
Kodak AA-400
Technique DWSI Screens
I. 0.1. Type DIN10-16
0.125 mm Pb
Radiation Source Ir.192
Source Size 3 mm C/J x 2 mm Sensitivity 2%
SFDjFFD 8" Density 2.3 to 2.5
RESULTS
JOINT # WELDER RADNO. OBSERVATION RESULT
SMAW + FCAW - PQR
6G 08 0-23 No recordable indications Acceptable
23 - 46 No recordable indications Acceptable
46 - 0 No recordable indications Acceptable
6G 78 0-23 No recordable indications Acceptable
23 - 46 No recordable indications Acceptable
46 - 0 No recordable indications Acceptable
I.•..'<I( \.. \~\..........~~.L o
-(10x40) 6 nos. REVIEWED
CA.WD F I!)~ "
tU €-~ 2.~B -~ •..•~
Signat itClient Re
R. VISW '-\Dp. -,
(Level II ,
IlWrs'!YRt892. Dubai. U.A.E. Tel: 04·457480 Fax: 04·452336 Tlx: 49591 LAB EMP.O. Box 26023. Abu Dhabi. U.A.E. Telephone: 02·261511 Telefax: 02·261512
~I.sl t'\o'\\ :~. ~o~'I'"n :..,-Su ~ovU\· :""~t:.f!!"~~t,.(~#4"';'·"_n\o\~ :..,-Su ·,,_n\o\\ :.j#,' .~.t:..I-~y'i n·~'1'",:""..r
![Page 8: WELDING PROCEDURE SPECIFICATION (WPS) Yes …](https://reader030.fdocuments.in/reader030/viewer/2022012711/61aaf535f08ebd6b0e16ca93/html5/thumbnails/8.jpg)
-iJ ~L' .al\ ~'.Jlo';11 p.: ~
!"mitates .:Jndusttial J!.a6otatot'lOilfield, Marine & Industrial Consultants Cernbcate No 943807
WELD PROCEDURE QUALIFICATION TEST REPORT Report#M 2973-1 P
Client: ElL Job Number 24100
Contech Eng. Co. LLC. Order Number Ref.: 28046l1SGSlbd99
P. 0 Box: 5750, Date Tested May 3,1999
Dubai, Test Code AWS D 1.1-98 & Client's Requirement
UAE. Tested By 2021204/132
Attention: Mr. S. G. Subramanian Equipment # Universal Tensile Machine, EIUMlO01
Identification219.1 x 12.7 mm Pipe Weld ProcedureMaterial: S 355 J2 H, Position: 6GJoint Type: Single 'V' - CJP, Welder Name: Mr. Anwar KhanWelder #W - 78, WPS: WPS/FCAW/99/01
ElL Sample #M 2973-1
TENSILE TESTS
Identification Dimensions Area Yield Yield Ultimate Tensile Fracture Elong. Red ofmm. Mm2 Load KN Strenath Load KN Strenath Location % Area
TI1 20.0 x 12.3 246.00 - - 131.0 533 N/mm2 On PM - -77,200 psi
- - - - - - - - - -
TI2 20.0 x 12.3 246.00 - - 130.0 528 N/mm2 On PM - -76,600 psi
- - - - - - - - - -
BEND TESTSType Mandrel Diameter Angle of Bend Test Result
Side Bend 1 38mm 1800 Satisfactory
Side Bend 2 " " SatisfactorySide Bend 3 . . SatisfactorySide Bend 4 . . Satisfactory
CHARPY 'V' NOTCH IMPACT TESTS (Joules)Test Temperature: Minus 20 °C Size: 10 x 10 x 55 mm
- - - - - - -Location WCL HAl - - - - - -Specimen A 48 172 - - - - - JSpecimen B 98 194 - - - - - JSpecimenC 94 120 - - - - - JAverage 80 162 - - - - - J
WELD MACROEXAMINATIONMacro -1 - - -
Satisfactory - - -NICK BREAK TEST ~",u'E~~
~o(O'y ~ ..~- - - ''+1/ ~~ '\P\
• III ~w- / •~ '.1?;:;::!!...'-. ,ting witnessed by: Mr. Lakshmana Rao (L~ Il."i:W ~
H.Uekar 11i~~' ~ ~ •..~~Senior Supervisor \ ,- . ~I ~ ~ Q Dale OT Issue. May 3,1999, B .~- ~ ~ / .n'
.~~~:~//~/ \~~ ~OlEIUMETlForm #03/Rev.O
~ ••~ , ~/-(~., j 'ej'"J' t/1 .~/ ,;:~ " ~
VUU<:;If" \\. '-: "t- ..0. Box6892, Dubai.U.A.E. Tel: 04·457480 Fax: IX: 49591 LABEM 0) r _\ :~. ~0 ~'('n:cr->li ~ oVU,· :.::..·r·t.·I- ...•.~INH ':"v"
.0. Box26023. Abu Dhabi,U.A.E. Telephone:02·261511 Telefax: 02·261512 L...0 \ ~ : \j. r.,n \ 0 \ \ :.j# . .1- ·",i n·~'(',:"...rpp
![Page 9: WELDING PROCEDURE SPECIFICATION (WPS) Yes …](https://reader030.fdocuments.in/reader030/viewer/2022012711/61aaf535f08ebd6b0e16ca93/html5/thumbnails/9.jpg)
•~_,cL· .aJ\ ~',l.o '11 -...:; oJ P.+
~mitat(!S' :JnJuS'ttia~ .iZa6oratot'lOilfield, Marine & Industrial Consultants Certrucare No 943807
WELD MACRO HARDNESS REPORT Report #M 2973-1 M1
Client: ElL Job Number 24100
Contech Eng. Co. LLC. Order Number Ref: 280451/SGS/bd99
P. 0 Box: 5750, Date Tested May 2,1999
Dubai, Test Code AWS 0 1.1-98 & Client's Requirement
UAE. Tested By 132
Attention: Mr.S.G. Subramanian Method Vickers Hardness Test HV 10 Kg
ElL Sample # M 2973-1 Equipment Vickers Hardness Tester
JOB DESCRIPTION 219.1 x 12.7 mm Pipe Weld Procedure, Position: 5G, Joint Type: Single 'V' - CJP,Welder Name: Mr. Anwar Khan, Welder #W - 78, WPS: WPS/FCAW/99/01
IMAXIMUMREADING II MACRO
10MATERIAL S 355 J2 H M1
- ,r- _. - - - ,
l - II' -,, - , - -
Sketch for illustration onlyAA BB CC DD EE FF GG HH " JJPM PM HAZ HAZ WELD WELD HAZ HAZ PM PM171 176 294 224 225 .212 292 216 164 176162 176 287 216 225 207 287 207 168 165175 165 252 213 268 207 230 202 160 157
REVIEWED
Date of issue: May 2, 1999
P.O. Box 6892. Dubai, U.A.E. Tel: 04·457480 Fax: 04·452336 Tlx: 49591 LAB EMP.O. Box 26023, Abu Dhabi, U.A.E. Telephone: 02·261511 Telefax: 02-261512
EIUMET/Form #04/Rev. 0
r1..s11'\0,\\ :~. ~o"rr, :.,rSU ~ov1A· :.;:..'r·t·Ld"A'"," '-;'.«r"
."_"1\0,," :~\j ."_"1\0\\ :':'yLJ.>' 'r·tl-~y'i n·"r.", .cr"
294
![Page 10: WELDING PROCEDURE SPECIFICATION (WPS) Yes …](https://reader030.fdocuments.in/reader030/viewer/2022012711/61aaf535f08ebd6b0e16ca93/html5/thumbnails/10.jpg)
•u/!"'---,cL' ed\ ~')~ ~ ~ : ..-'f!.
!...mitat(ls :JnJusttia~ .i!.a6ot.atot'lOilfield, Marine & Industrial Consultants Certificate No 943807
ElL Sample #M 2973 M1219.1 x 12.7 mm Pipe Weld Procedure
Material: S 355 J2 H,Position: 6G
Joint Type: Single 'V' - CJP,Welder Name: Mr. Anwar Khan
Welder #W - 78,WPS: WPS/FCAW/99/01
P.O. Box 6892, Dubai, U.A.E. Tel: 04·457480 Fax: 04·452336 Tlx: 49591 LAB EMP.O. Box 26023, Abu Dhabi, U.A.E. Telephone: 02·261511 Telefax: 02·261512
rl..sl~"o,,\:~ ~o"'rn:..,..fu ~OVU\':';;' '1".(.I_..r.'''I''''''", ...,.,."_'1'1\0,," :..,..fu ."_'1'1\0\\ :.j# ·r·t·I-~yi n·"'r,,, ...,.,