Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head...
Transcript of Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head...
![Page 1: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/1.jpg)
©Nucleom inc.Used Fuel Containers NDE Inspection Program Report
![Page 2: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/2.jpg)
2 NDT in Canada 2017 Conference (June 6-8, 2017)
- Historical Context
- NWMO – Role and Responsibilities
- What is Canada’s Used Nuclear Fuel?
- National Infrastructure Project
- NDE Design and Development
- Results
- Partial Penetration Weld Inspection Program
- Copper Coating Inspection Program
- Conclusion
Agenda
![Page 3: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/3.jpg)
©Nucleom inc.©Nucléom inc.
Historical Context
![Page 4: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/4.jpg)
4 NDT in Canada 2017 Conference (June 6-8, 2017)
NWMO – Role and Responsibilities
• NWMO: Nuclear Waste Management Organization (https://www.nwmo.ca)
• Formed in 2002 as required by the Federal Nuclear Fuel Waste Act (NFWA)
• Funded by Canada’s nuclear energy corporations as required by the NFWA
• Operates on a not-for-profit basis
NWMO’s mission is to develop and implement collaboratively with Canadians, a management approach for the long-term care of
Canada’s used nuclear fuel that is socially acceptable, technically sound, environmentally responsible, and economically feasible.
![Page 5: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/5.jpg)
5 NDT in Canada 2017 Conference (June 6-8, 2017)
What is Canada’s Used Nuclear Fuel?
• It is the result of using uranium to produce electric power in a nuclear reactor.
• It is typically a solid ceramic, encased in Zircaloy metal tubing.
• It is constantly generating heat, about 3-10 W per bundle, similar to an LED lightbulb.
• It contains high levels of radioactivity.
Fresh fuel
Uranium dioxide (UO2) 100%
Used CANDU fuel
Uranium dioxide (UO2) 98.5%
Non-radioactive products 1.0%
Radioactive products 0.5%
![Page 6: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/6.jpg)
6 NDT in Canada 2017 Conference (June 6-8, 2017)
Over 2.6 Million Fuel Bundles Safely Stored
![Page 7: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/7.jpg)
7 NDT in Canada 2017 Conference (June 6-8, 2017)
National Infrastructure Project
![Page 8: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/8.jpg)
8 NDT in Canada 2017 Conference (June 6-8, 2017)
Used Fuel Container
![Page 9: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/9.jpg)
9 NDT in Canada 2017 Conference (June 6-8, 2017)
Used Fuel Container
Steel Shell
• Nuclear pressure vessel grade steel
• A/SA-106 Gr. C NPS 22” SCH 140 Seamless Steel Pipe
Steel Hemi-Head
• Nuclear pressure vessel grade steel
• A/SA-516 Gr.70 plate, hot-formed
Welding
• Hybrid Laser Arc Welding (HLAW)
![Page 10: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/10.jpg)
10 NDT in Canada 2017 Conference (June 6-8, 2017)
Used Fuel Container
SHELL HEAD
![Page 11: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/11.jpg)
11 NDT in Canada 2017 Conference (June 6-8, 2017)
Used Fuel Container
Electrodeposition for main body• Reverse galvanic cell• Nano-crystalline coating
Cold spray for Closure Weld Zone• Solid state high-speed spray
of copper particles
Copper Coating
![Page 12: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/12.jpg)
12 NDT in Canada 2017 Conference (June 6-8, 2017)
Used Fuel Container
Final Product
![Page 13: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/13.jpg)
©Nucleom inc.©Nucléom inc.
NDE Design and Development
![Page 14: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/14.jpg)
14 NDT in Canada 2017 Conference (June 6-8, 2017)
Define inspection techniques to achieve 100% coverage within applicable codes of all critical components at different stages of UFC
manufacturing for increase reliability of the long storage life.
NDE Design and Development
Partial Penetration Weld Program Copper Coating Program
![Page 15: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/15.jpg)
15 NDT in Canada 2017 Conference (June 6-8, 2017)
NDE Design and Development
INPUTComponent Geometry, Material Characteristics
Review of Codes and
Standards Requirements
Sample List
Preliminary Target
Flaw Size ReportReview of Potential
Inspection Techniques
Technology
Matrix
Inspection
Techniques Selection
Definition of Inspection
Configurations
Data Acquisition and
Analysis
UT and ECT
Data Files
Optimization of Inspection
Configuration
Data Analysis Report &
PoD Analysis Inputs
Specifications of Selected
Examination Methods
Final Inspection
Procedures Target Flaw Size Definition &
Statistical Relevance
Program Report
Modeling and
Calculations
PoD Analysis
Flaw Manufacturer
Capabilities Assessment
Used Fuel Container NDE Design & Development
Flowchart
![Page 16: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/16.jpg)
16 NDT in Canada 2017 Conference (June 6-8, 2017)
NDE Design and Development
Used Fuel Container Manufacturing Stages
![Page 17: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/17.jpg)
©Nucleom inc.©Nucléom inc.
Results: Partial Penetration Weld
![Page 18: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/18.jpg)
18 NDT in Canada 2017 Conference (June 6-8, 2017)
Partial Penetration Weld
SHELL HEAD
Area of Interest:• Manufacturing flaws• Depth of the Penetration
![Page 19: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/19.jpg)
19 NDT in Canada 2017 Conference (June 6-8, 2017)
Partial Penetration Weld
Looking for:• Surface connected defects• In-volume cracks/porosities• Weld penetration depth
![Page 20: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/20.jpg)
20 NDT in Canada 2017 Conference (June 6-8, 2017)
Partial Penetration Weld
TOFD
Angle Beam - SW
0°LW
ECACombination NDE Techniques
![Page 21: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/21.jpg)
21 NDT in Canada 2017 Conference (June 6-8, 2017)
Partial Penetration Weld
100% Detection
![Page 22: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/22.jpg)
22 NDT in Canada 2017 Conference (June 6-8, 2017)
Partial Penetration Weld• Real Welding Defects (On-Purpose)
![Page 23: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/23.jpg)
©Nucleom inc.©Nucléom inc.
Results: Copper Coating
![Page 24: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/24.jpg)
24 NDT in Canada 2017 Conference (June 6-8, 2017)
Copper Coating
Copper Coating Thickness : ~4.5mm
Electrodeposition Cold Spray
Copper/Carbon Steel Interface Signal
~23dB Amplitude Delta between Coating Techniques
![Page 25: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/25.jpg)
25 NDT in Canada 2017 Conference (June 6-8, 2017)
Copper Coating
Copper Coating
Carbon Steel
Wedge
UT Beams
~4mm
Looking for:• Surface connected defects• In-volume porosities• Bonding issues with carbon steel• Coating thickness
![Page 26: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/26.jpg)
26 NDT in Canada 2017 Conference (June 6-8, 2017)
Copper Coating
Hole Id Diameter Measured Diameter Measurement Delta
1 3/64” (1.2mm) -- --
2 3/32” (2.4mm) 3.0mm 0.6mm
3 9/64” (3.6mm) 5.00 1.4mm
4 7/32” (5.6mm) 7.0mm 1.4mm
5 21/64” (8.3mm) 10.0mm 1.7mm
6 29/64” (11.5mm) 13.0mm 1.5mm
7 1-1/32” (26.2mm) 27.0mm 0.8mm
• Bonding Issues
5MHz, 128 el. (Aperture: 16el.) – Linear Scan
![Page 27: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/27.jpg)
27 NDT in Canada 2017 Conference (June 6-8, 2017)
Copper Coating• Samples with FBH (Electrodeposited and Cold Sprayed Coating)
![Page 28: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/28.jpg)
28 NDT in Canada 2017 Conference (June 6-8, 2017)
Copper Coating• SDH of the Same Samples (Electrodeposited and Cold Sprayed Coating)
FBH
![Page 29: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/29.jpg)
29 NDT in Canada 2017 Conference (June 6-8, 2017)
Copper Coating• Typical UT Results (Straight Beam - Electrodeposited Copper)
![Page 30: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/30.jpg)
30 NDT in Canada 2017 Conference (June 6-8, 2017)
Copper Coating• Typical UT Results (Straight Beam - Electrodeposited Copper)
![Page 31: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/31.jpg)
31 NDT in Canada 2017 Conference (June 6-8, 2017)
Copper Coating• Typical UT Results (Straight Beam - Electrodeposited Copper)
![Page 32: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/32.jpg)
32 NDT in Canada 2017 Conference (June 6-8, 2017)
Copper Coating• Typical UT Results (Straight Beam - Cold Sprayed Copper)
![Page 33: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/33.jpg)
33 NDT in Canada 2017 Conference (June 6-8, 2017)
Copper Coating• Typical ECA – Low Frequency Probe (In-Volume Features – SDH and FBH)
![Page 34: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/34.jpg)
34 NDT in Canada 2017 Conference (June 6-8, 2017)
Copper Coating• Typical ECA – Low Frequency Probe (Surface Breaking Features)
=0.5mm
=1.0mm
=1.5mm
=3.0mm
0xCT ¼xCT ½xCT ¾xCT
x1.0mm
x1.0mm
x0.3mm x0.5mm x1.0mm x2.0mm
x0.3mm
x0.5mm
x1.0mm
x2.0mm
![Page 35: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/35.jpg)
35 NDT in Canada 2017 Conference (June 6-8, 2017)
Copper Coating
Cold Spray
Electrodeposition
• Coating Thickness (Part 1)
Interface Signal Amplitude
![Page 36: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/36.jpg)
36 NDT in Canada 2017 Conference (June 6-8, 2017)
Coating Thickness Demonstration Sample
Copper Coating
![Page 37: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/37.jpg)
37 NDT in Canada 2017 Conference (June 6-8, 2017)
Copper Coating
Cold Spray
Electrodeposition
• Coating Thickness (Part 2)
Carbon Steel Back-Wall Signal Monitoring
(0° LW Examination)
Thicker (4mm Coating) Thinner (0.5mm Coating)
![Page 38: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/38.jpg)
38 NDT in Canada 2017 Conference (June 6-8, 2017)
Copper Coating
Cold Spray
Electrodeposition
4mm 3mm 2.5mm 2mm 1mm 0.5mm
0.5 mm
2 mm
2.5 mm3 mm
4 mm
1 mm
• Coating Thickness (Part 3)
![Page 39: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/39.jpg)
39 NDT in Canada 2017 Conference (June 6-8, 2017)
Copper Coating• Coating Thickness (Part 4)
![Page 40: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/40.jpg)
©Nucleom inc.©Nucléom inc.
Conclusions
![Page 41: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/41.jpg)
41 NDT in Canada 2017 Conference (June 6-8, 2017)
• Identified NDE Techniques
• Partial Penetration Weld
• Copper Coating
• Identified the Challenges
• NDE System Specifications
Conclusion
![Page 42: Used Fuel Containers NDE Inspection Program Report · Seamless Steel Pipe Steel Hemi-Head •Nuclear pressure vessel grade steel •A/SA-516 Gr.70 plate, hot-formed ... •Reverse](https://reader035.fdocuments.in/reader035/viewer/2022070713/5ed00777c8a226618b16e5d7/html5/thumbnails/42.jpg)
42 NDT in Canada 2017 Conference (June 6-8, 2017)
Question