STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service...
Transcript of STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service...
![Page 1: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/1.jpg)
Steel Academy Steel Institute VDEh PO box 104842 40039 Düsseldorf Sohnstraße 65 40237 Düsseldorf Germany Fon +49 211 6707 454 Fax +49 211 6707 655 E-Mail: [email protected] Internet: www.steel-academy.com
STEEL TEEMING LADLE: Ladle Metallurgical Treatment / Refractory Stress / Materials and
Lining Concepts
Dipl.-Ing. Hans-Christian Schröter Hüttenwerke Krupp Mannesmann GmbH, Duisburg
and Ing. Andreas Viertauer
RHI AG, Wien
Seminar:
Refractory Technology – Applications, Wear Mechanism, Failures
![Page 2: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/2.jpg)
VDEh Stahl AcademyVDEh Stahl AcademyRefractory - Technology
Applications, Wear Mechanism and Failures
Steel Teeming Ladle:
Ladle Metallurgical Treatments / Refractory Stress / Materials and Lining Concepts
Stahl-Zentrum1 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Content
Metallurgical Tasks Steel Production overview
Example: ULC, HIC, TRIP, TWIP
Secondary Metallurgy Tasks
Aggregates vs. Refractories
Ladle slag
Purging instrumentation
Teeming ladleTeeming ladle Lining concepts
Wear mechanism
Lab investigation
D i d h ti Drying- and heating
Laser- vs. Thermo vision Scan
Purging
„Problem areas“ and Check list
Stahl-Zentrum2 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Outlook and Summary
![Page 3: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/3.jpg)
From Ore to Steel
Stahl-Zentrum3 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
What is steel? For Definition see Fe – Fe3C Diagram
Stahl-Zentrum4 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
![Page 4: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/4.jpg)
Metallurgical Tasks – Automotive Industrythe 50th Nowthe 80th
Chemical Composition: [C] ~ 0,10 % [C] ~ 0,05 % [C] ≤ 0,0030 (≤ 0,0015) % [C] 0,10 %
[P] < 0,030 %
[S] < 0,030 %
[N] ≤ 0 0090 %
[C] 0,05 %
[P] ≤ 0,020 %
[S] ≤ 0,020 %
[N] ≤ 0 0060 %
[C] ≤ 0,0030 (≤ 0,0015) %
[P] ≤ 0,010 (≤ 0,008) %
[S] ≤ 0,010 (≤ 0,008) %
[N] < 0 0035 %
Prozess Route Steel Plant:
[N] ≤ 0,0090 % [N] ≤ 0,0060 % [N] < 0,0035 %
[Ti]-, [Nb]-, [B]- alloyed
OHF; Ingot casting LD/ EAF; Treatment stand,CCM
LD-S/ EAF; LF, CASOB,VD-OB RH-OB; CCM
Stahl-Zentrum5 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
CCM VD-OB, RH-OB; CCM
Metallurgical Tasks – Offshore Industry
LD-S/ EAF - RH/VD – CCM[S] ≤ 0,0010 (≤ 0,0005) %[P] 0 0080 ( 0 0060) %
API- HIC* Grade:
[P] ≤ 0,0080 (≤ 0,0060) %[H] ≤ 0,0002 (≤ 0,0015) %[N] ≤ 0,0060 (≤ 0,0040) %
Stahl-Zentrum6 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
*API- HIC: American Petroleum Institute- Hydrogen Induced Cracks
![Page 5: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/5.jpg)
Metallurgical Tasks – Automotive Industry
TRIP* Grade:LD-S/ EAF – (Induction Furnace) –
TWIP* Grade:
LD-S/ EAF – Induction Furnace –RH/VOD – CCM[Al] ~ 1 %[Mn] ~ 2 - 15 %[P] < 0,010 %S %
RH/VOD – CCM[Al] ~ 5 %[Mn] ~ 20 %
Stahl-Zentrum7 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
[S] < 0,0030 %*TRIP: Transforming Induced Plasticity *TWIP: Twinning Induced Plasticity
Material Properties
Stahl-Zentrum8 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
![Page 6: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/6.jpg)
Metallurgical Tasks
Adjustment of the needed chemical composition and steel temperature Adjustment of the needed chemical composition and steel temperature
Deoxidation and removal of non metallic inclusions (NMI)
Desulphurization de [S]
Degassing de [H]
de [N][ ]
Decarburization de [C]
„Clean Steel“
Stahl-Zentrum9 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Aggregates for Secondary Steel Making
Stahl-Zentrum10 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
![Page 7: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/7.jpg)
H ti d [S] Clean- d [C] d [N]d [H]Modifi-
Metallurgical tasks in detail
LT
Heating de [S] Cleanliness de [C] de [N]de [H]Modifi
cation
LF
CAS-OB
RH OBRH OB
VD VOD
Stahl-Zentrum11 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Technical Data from a LF for 160 t 2 Ladle transfer cars Primary voltage 30 kV Transformer power 22 MVA Secondary power 45 kA, 160 - 330 V Electrode diameter 457 mm Heating rate 3 - 5 °C/min Energy consumption 10 - 30 kWh/t Spec. heating consumption 0,5 kWh/t °C Electrode consumption 6 10 g/kWh Video I Electrode consumption 6 – 10 g/kWh Purging facilities (regulation unit, docking stations) Wire feeding for Al, CaSi, FeTi and other Desulphurization with powder (CaSi, CaC2, Lime)
Video I
Desulphurization with powder (CaSi, CaC2, Lime) Manipulator for temperature and sample Alloying system- Bunker system Dedusting unit
Stahl-Zentrum12 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source Fotos: SIEMENS-VAIVideo II
![Page 8: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/8.jpg)
LF- treatment steps
Stahl-Zentrum13 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Ladle Furnace versus Ladle Wear
Thermal radiation during arcing Not efficient bottom stirring Splashes of steel and slag Short- circuit esp. for the purging plugs Overheated slag Less slag
Covering the electric arc with slag Enough amount of slag with less oxides Enough amount of slag with less oxides Optimal length of the arc Correct symmetry of the 3 phases Small electrode circle
Stahl-Zentrum14 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Small electrode circle Effective ladle purging unit SMS
![Page 9: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/9.jpg)
Chemical Heating – CAS-OB, HALTTreatment tasks: Fast Temperature adjustmentast e pe atu e adjust e t Homogenization Alloying Deoxidation Desulphurization Removal of non metallic inclusions
Stahl-Zentrum15 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
CAS-OB versus Ladle Wear
Aluminothermy heating Splashes and build up of steel and slag on/ into the bell Overheated Slag ( bad stirring and or too long heating) Bad slag chemistry- Less slag – too much carry over
slag (high (FeO)slag (high (FeO)
Enough amount of slag with less oxides Enough amount of slag with less oxides optimized Slag metallurgy
Effective bottom stirring
Stahl-Zentrum16 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
![Page 10: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/10.jpg)
Comparison LF versus CAS-OB
LF CAS- OB
Heating rate [K/min] 3 - 5 7 - 10
Energy consumption [kWh/t K] 0,4 -
Oxygen consumption [Nm3/t K] - 0,03
Aluminium consumption [kg/t K] - 0,04
Refractory consumption bell [kg/ t Steel] - approx. 0,15
Oxygen lance - yes
Graphite electrode consumption [g/kWh] 6 - 10 -
Investment high low
Stahl-Zentrum17 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Steel Grades and Carbon Content
%<
0,02
5 %
ent i
f C <
m T
reat
mVa
cuum
Stahl-Zentrum18 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
![Page 11: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/11.jpg)
Vacuum Plant NomenclatureRecirculation Processes
DH D d Hö d ( d RH) DH Dortmund Hörde (revamped to RH)
DH-OB Dortmund Hörde - Oxygen Blowing (revamped to RH)
RD Recirculation Degasser
RH Ruhrstahl Heraeus
RH-OB Ruhrstahl Heraeus - Oxygen Blowing (standard)
RH-OTB Ruhrstahl Heraeus - Oxygen Top Blowing (same as RH-KTB)
RH-KTB Ruhrstahl Heraeus - Kawasaki Top Blowing
VCP Vacuum Circulation Process
VCP-O Vacuum Circulation Process - Oxygen Blowing
Non-Recirculation ProcessesVOD V O D i (d C d ) VOD Vacuum Oxygen Degassing (deC under vacuum)
VD-OB Vacuum Degassing (standard), OB under atmospheric pressure
VAD Vacuum Arc Degassing
Which type fits is depend on the product mix!
Stahl-Zentrum19 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Which type fits is depend on the product mix!
RH-Degasser (Ruhrstahl - Heraeus)
Core equipment Vacuum system: Mechanical Pumps and/or
Steam Injectors Burner: Natural gas and Oxygen, 50 K/hg yg , Snorkel: Lift gas Ar/N2 up to 2000 Nl/min Oxygen Lance: Heating, Desculling and
fine adjustment of [C]/a[O] ratiofine adjustment of [C]/a[O] ratio Alloying Equipment Lifting System: Vessel, ladle or transfer car Service Equipment: Desculling & Gunning Service Equipment: Desculling & Gunning Lowest pressure: 0,5 mbar
Stahl-Zentrum20 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
![Page 12: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/12.jpg)
RH- Process Homogenization A deep impulse of steel flow back into the ladle is a precondition forinto the ladle is a precondition for a good homogenization!Take care for:1. To be as deep as immersed with
the snorkels!2 The number of working lift gas2. The number of working lift gas
tubes are important!3. Monitor Ar- lift gas flow and
pressure for each line!4. Operate with a single lift gas
regulation system!
Stahl-Zentrum21 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
RH-Degasser and Refractory Wear
St l d l h i t (HIC ULC) Steel and slag chemistry (HIC, ULC) Long treatment time (> 30 minutes) Long or short heat sequences Thermal stress
Ai t i t t th fl ( k l l) Air entrainment at the flanges (snorkel-vessel) Vessel build up – deskulling with O2- lance
RH logistic (sequence length, maintenance cycle,..) Optimal snorkel treatment (deskulling, gunning) Perfect maintenance and refractory service Balanced refractory liningBalanced refractory lining
Stahl-Zentrum22 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM22
![Page 13: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/13.jpg)
Snorkel Deskulling Facilities
The skull removal facility isThe skull removal facility is, An excavator A special frame which is located on a service car or on a frame which will be settled onto the ladle
transfer car
Stahl-Zentrum23 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
After the scull removal is done gunning should happen!!!!
Snorkel gunning
Manual Manipulator+ = PERFECT
BAD
Stahl-Zentrum24 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Video
![Page 14: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/14.jpg)
RH- degasser possible life time for each partPart Life time (heats)Snorkels and legs 80 300Snorkels and legs 80 - 300
Vessel lower part ~ 300 (600)
Vessel upper part > 3.000
Alloying chute > 3.000Alloying chute > 3.000
Top head (elbow) > 6.000
Gunning consumption [kg/t] 0,6 – 1,5
Stahl-Zentrum25 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Vacuum Tank Degasser (VD, VD-OB, VOD)
120 120 t VOD Plant Shanghai No.1, Start t VOD Plant Shanghai No.1, Start UpUp 20042004 1 Heat 4 Alloying System
2 Tank 5 Purge PlugSource: left: SMS Mevac, Symposium Moscow July 2004; right: MARTI Technology
Stahl-Zentrum26 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
3 Oxygen Lance
![Page 15: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/15.jpg)
Purging – HKM VD key figures
System: 2x bottom purging plug
Pressure: 14 bar (max.)
Flow rate: 2x1200l/min (max.)
Emergency strategy: lance stirring
Degassing: 5‘ atm. – deep vacuum (5 mbar), reduced flow rate
Vacuum treatment: 20‘, max. flow rate
Slopping: wet slags (O2-rich) beginning at 500-50 mbar
Slopping detection: camera on bathSlopping detection: camera on bath
Reaction on slopping: counter flooding
Total stirring gas: >16.000l
Stahl-Zentrum27 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
Tank Degasser VD/VD-OB/VOD
Intensive metal-slag reaction! High erosion esp. slag line High thermal stressg Built up and slashing Spontaneous boiling reaction Slag chemistry (eg. MgO-, CaF2- content)
Enough free- board Controlled vacuum pump down curve Controlled vacuum pump down curve Efficient and controlled bottom stirring Convenient bricks for the slag line CaF2- free If MgO bricks MgO slag saturation
Stahl-Zentrum28 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
If MgO- bricks MgO- slag saturationSource Photo: 100 t VD- twin Degasser Handang, China
![Page 16: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/16.jpg)
VD- Process and Control Purging
Stahl-Zentrum29 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Link Video
Comparison RH/RHOB - VD/VODRH - RHOB VD - VOD
Furnace LD, EAF* EAF, LD*
Product flat, some times long* long, some times flat*
Steel grades ULC, SULC, HIC, Plates, Pipes HIC, Plates, Pipes, ULC*
Freebord [mm] 300 - 400 500 - 1500
Ladle shell temperature less higherLadle shell temperature less higher
Ladle life time 100% approx. 60 - 80 %
Treatment time [min] 20 - 40 20 - 45 (VOD up to 120)
Lenght of a sequence Snorcel wear no limit, especially TWIN
R f t ti [k /t] 0 45Refractory consumption [kg/t] approx. 0,45 -
Gunning consumption [kg/t] approx. 0,5 - ''
Slag metallurgy no S; P,Si,Mn,Cr
Desulphurisation no < 10 ppm
Decarburisation < 15 ppm in 15-17 min < 20 - 30 ppm in 25 min
Degassing [H] in 20 min < 1,5 ppm < 1,5 ppm
Degassing [N] in 20 min < 40 ppm < 30 ppm
Temperature losses [K/min] 0,8 - 1,5 2,0 (250 t) bis 4,5 (bei 10 t)
Stahl-Zentrum30 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Investment high lower
![Page 17: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/17.jpg)
Chemical Reactions in a Steel Teeming ladle
Stahl-Zentrum31 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: M. W. Egger; Diploma Thesis; Steel Desulphurization, Montan University Leoben; 2005.
Chemical Reactions between Metal- Slag Interface / Slag
Direction of mass transport
/ liquid Steel
p
Chemical Reactions between Metal-Slag-Interface:
Stahl-Zentrum32 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM32
Source: H. Lachmund et al; Steel Research 74 (2003) No. 2, S 77-85
![Page 18: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/18.jpg)
%
Desulphurization Efficiency and Ladle Refractory
on in
%hu
risat
iD
esul
p
Stahl-Zentrum33 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: Kosmider et al, Stahl u. Eisen 1999 Nr. 22, 1215-1221
Each grade has in principle their own slag compositionBasicity
Steel Grade FeO SiO2 MnO CaO MgO Al2O3 P2O5 S TiO2 Cr2O3CaO/(Al2O3+SiO
2) Lime Alumina MgO SiO2
Tapping
Steel Grade FeO SiO2 MnO CaO MgO Al2O3 P2O5 S TiO2 Cr2O3 2) Lime Alumina MgO SiO2
ULC- IF 17 7,5 12 20 11,5 30 0,40 0,02 1,3 0,3 0,53 0 (x) X X 0
Drawing 5,4 5,6 3,9 38 13,7 33,1 0,04 0,06 0,2 0,1 0,98 X X X 0
Steel Desulphurised 0,7 8,5 0,2 52,4 9,2 28,6 0,00 0,20 0,2 0,0 1,41 X X X 0* p , , , , , , , , , , , X X X 0
Wire without Al 2,7 45,0 5,0 35,0 8,0 4,0 kA 0,05 0,1 0,71 X 0 X X
Rails, Welding Wire < 1,5 34,0 2,0 46,0 8,0 7,0 kA 0,05 1,12 X 0 X X
Wire with Si, low requirements 6,0 14,0 7,0 44,0 10,0 15,0 kA 0,05 1,52 X 0 X 0
(X)= some plants
requirements
Wire without Si 6,6 8,0 3,0 55,0 8,0 21,0 0,04 0,20 1,90 X X X 0
Rails 2,7 14,0 1,0 42,0 11,0 29,0 0,04 0,20 0,98 X X X 0
What ‘s about Fluorspar/ CaF2 ?
* All grades for Ca- metallurgy (e.g.. Cast- ability for thin slab caster),steel cleanliness, MgO- and CaO saturation,……..
Source: All data from VDEh membersp 2
Stahl-Zentrum34 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: 2013 04 VDEh Steel Academy Refractory Technology II, Ladle Metallurgical Treatments & Refractory Stress for a Steel Teeming Ladle
![Page 19: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/19.jpg)
Slags in the CaO – SiO2 – Al2O3 Diagram
Stahl-Zentrum35 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Fotos: Dillinger Hütte, Salzgitter, Marienhütte
Basic- and acid slags in the CaO – SiO2 – Al2O3 Diagram
Stahl-Zentrum36 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Deutsch, BHM 1995, Paper # 11
![Page 20: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/20.jpg)
CS- and CA- Slags at the CaO – SiO2 – Al2O3 Diagram
Stahl-Zentrum37 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: C. Brüggmann, J. Pötschke; Contribution to the slagging of MgO in secondary metallurgical slags, September 8th and 9th 2010, Refractory Colloquium Aachen, Germany
Influence of Steel Temperature and MgO- saturation30
% 1700°C
30
% 1700°C
20
25
g in
Mas
s-%
d 17
00°C
1600°C
20
25
g in
Mas
s-%
d 17
00°C
1600°C
15
20
of L
adle
Sla
gr 1
500°
C a
nd
1500°C15
20
of L
adle
Sla
gr 1
500°
C a
nd
1500°C
10
Satu
ratio
n o
alcu
late
d fo
r
10
Satu
ratio
n o
alcu
late
d fo
r
0
5
0 5 10 15 20 25 30
MgO
-S ca
0
5
0 5 10 15 20 25 30
MgO
-S ca
Stahl-Zentrum38 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
0 5 10 15 20 25 30
MgO-Saturation in M-%0 5 10 15 20 25 30
MgO-Saturation in M-%Source: Schürmann Formula for furnace slag
![Page 21: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/21.jpg)
MgO- saturation – as an example (Steel Plant X)
Start LF End LF
Stahl-Zentrum39 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: Park, J.M. und K.K. Lee: Reaction Equilibrium between liquid iron and CaO-Al2O3-MgO; Steelmaking Conference Proceedings (1996), 165-166.
MgO- saturation and some different Steel Grade Slags
Drawing Grade
HIC, Pipe Grades
Slag
ULC
Stahl-Zentrum40 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: Steel Academy, Refractory Technology Part II, 2008 Secondary Metallurgy and Ladle Refractory Stress
![Page 22: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/22.jpg)
Th ti l M O l bilit i CAS l 9% ( P k L Di )
HKM - MgO- ladle slag saturation method
Theoretical MgO-solubility in CAS-slags ~ 9% ( see Park Lee Diagram)
Addition of dolomite to prevent wear of lining.
But:
Slag forming by oxidation of aluminium + lime- and dolomite-addition takes time!
During dissolving lime and dolomite also MgO from the lining gets dissolved.g g g g g
Stahl-Zentrum41 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
Comparison of Slag Retaining Systems
18
16
14[kg/
t]
12
10
8y O
ver S
lag
6
4
2
Car
ry
0
Without FloatingTetrahedron
FloatingBall
PneumaticStopper
Gas Impinging
FloatingDart
Slag detection + Converter Slide Gate
Stahl-Zentrum42 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Slide Gate
![Page 23: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/23.jpg)
Inductive- vs. RH-steel flow
Stahl-Zentrum43 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: 2007 VDEh Steel Academy Refractory Technology II, Ladle Metallurgical Tratments & Refractory Stress for a Steel Teeming Ladle
Steel flow lance vs. Bottom stirringBottom stirring Lance stirring
Dead area
Stahl-Zentrum44 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: 2007 VDEh Steel Academy Refractory Technology II, Ladle Metallurgical Treatments & Refractory Stress for a Steel Teeming Ladle
![Page 24: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/24.jpg)
Strömungsverteilung
Stahl-Zentrum45 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: W. Pluschkell; Stahl und Eisen 101 [1981), S 97/103
Different Plugs
Stahl-Zentrum46 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: Flyers Product Info from different plug suppliers
![Page 25: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/25.jpg)
Purging Plug LocationVersion# 1 Version# 2
Version# 3 Version# 4Version# 3 Version# 4
Stahl-Zentrum47 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: 2015, RHI Technology Center Leoben, CFD Simulation- Case study Ladle Purging
Cross section and top view of velocity pattern for one and 2 Plugs with differentCross section and top view of velocity pattern for one and 2 Plugs with different locations 400 lit/min
Version 1 Version 2 Version 3 Version 4
Stahl-Zentrum48 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: 2015, RHI Technology Center Leoben, CFD Simulation- Case study Ladle Purging
![Page 26: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/26.jpg)
Thoroughly distribution of Alloying material
14
10
12
teria
l [m
³]
6
8
g al
loyi
ng m
a
V1V2V3
2
4
volu
me
faci
n V3V4
0
2
0 50 100 150 200 250 300Time [sec]
Stahl-Zentrum49 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: 2015, RHI Technology Center Leoben, CFD Simulation- Case study Ladle Purging
Soft Stirring and bubble size formation
small bubbles large bubbles
Stahl-Zentrum50 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
![Page 27: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/27.jpg)
Experimental Procedure
Water tank 1000 l
Pressure valve
with mass flow
ll
Range 0,5 – 10 l / min
controller
High speed
camera 50 frames per second
Image processing
software
Automated bubble
counting
Determination of
bubble
dimensions
Averaging of 500 frames
for each flow rate
Stahl-Zentrum51 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: B. Trummer et al, Water Modelling Comparison of Hybrid – Slot- and Porous Plug Designs, UNITECR 2015, Vienna,
Water modeling resultsBubble formation of hybrid- porous- and slot plugFl t 10 l/ i
hybrid porous slot Flow rate: 10 l/min
Stahl-Zentrum52 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: B. Trummer et al, Water Modeling Comparison of Hybrid – Slot- and Porous Plug Designs, UNITECR 2015, Vienna,
![Page 28: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/28.jpg)
Steel Cleanliness and Soft bubbling 0,2 lit Ar x min-1 x t Steel-1
] tot
ppm
[O
Remaining [O] tot
Stahl-Zentrum53 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: Neifer, Rödl, Bannenberg, Lachmund; Stahleisen 117 (1997), Nr 5, S 55/63
Soft bubbling time min
[O] tot over several process steps
-%[O
] tot
Mas
s-[
LF RH Soft BubblingCaSi Wire Casting
Stahl-Zentrum54 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: A. Gantner, VDEh Seminar Sekundärmetallurgie; Metallurgie des Pfannenofens , 24.10.2012
![Page 29: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/29.jpg)
Ladle stirring system
Control room PC / HMI
Control Panel
Gas control boxGas control box
Level2/3
Ar / N2
Stahl-Zentrum55 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: R. Ehrengruber, Excellence Intelligence Gas Control Systems; 2014 ECCC Graz
Purging Visualization L1 control room and docking station
IEM
ENS-
VAI
cou
plin
g fly
er S
Source: voestalpine Stahl Linz
Sour
ce: G
as
Stahl-Zentrum56 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: 2007 VDEh Steel Academy Refractory Technology II, Ladle Metallurgical Tratments & Refractory Stress for a Steel Teeming Ladle
![Page 30: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/30.jpg)
Purging instrumentation and visualization at L1
ubop
timal
Su
Stahl-Zentrum57 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: 2013 04 VDEh Steel Academy Refractory Technology II, Ladle Metallurgical Treatments & Refractory Stress for a Steel Teeming Ladle
% Lance Stirring and different Line Pressure13.0 [bar][bar]
35
40
45
12 [bar] 13.5 [bar] 12.8 [bar]
20
25
30
35
urgi
ng
10
15
20
% L
ance
p
0
5
period under review
Stahl-Zentrum58 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: Viertauer, Exenberger 2003, 14th IAS Steelmaking Conference San Nicolas, Argentina; Efficient Ladle Management at voestalpine Stahl
![Page 31: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/31.jpg)
Purging – Paul-Wurth coupling device steel ladle
Stahl-Zentrum59 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
Purging – Paul-Wurth coupling device VD-Stand
Stahl-Zentrum60 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
![Page 32: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/32.jpg)
Purging – installation and performance data
Purge plug + well block set Replacement purge plug with sleevePurge plug + well block setLadle age 0-19/21; lifetime 21 heats
Replacement purge plug with sleeve Ladle age >21; lifetime 12 heats
Stahl-Zentrum61 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
Purging - visualization
Stahl-Zentrum62 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
![Page 33: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/33.jpg)
Purging – validation of purging performance
Stahl-Zentrum63 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
Purging – validation of purging performance
Stahl-Zentrum64 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
![Page 34: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/34.jpg)
Purging – validation of purging performance
Stahl-Zentrum65 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
Purging – validation of purging performance
Stahl-Zentrum66 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
![Page 35: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/35.jpg)
Item System Info Life time
HKM - Ladle Performance Data Functional Products
Item System Info (heats)Flow control CS100 Bore size 80mm
Max. 300 minSlide gate plates 81.3% Al2O3, 10.9% SiO2, 5.4% ZrO2,
7.2% C
Max. 300 min casting = approx.3,1
D i l 85.0% Al2O3, 8.0 % SiO2, 4.0% ZrO2, 2 1Drain nozzle 85.0% Al2O3, 8.0 % SiO2, 4.0% ZrO2, 2.0 % CaO, 0.5% MgO , 4.0% C 2,1
Inner nozzle 91.8% Al2O3, 0.1% Fe2O3, 0.1% SiO2, 2.4% CaO, 5.6 % MgO 9
Purging plugs Multiport 12 x 0,15 x 2mm / 12 x 0,2 x 2mm Max. 21 (set)/ 12 (repl.)
Double-HP 0,2mm Max. 21 (set)/ 12 (repl.)
Stahl-Zentrum67 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
Purging – reasons for failure
Stahl-Zentrum68 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
![Page 36: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/36.jpg)
HKM - Ladle disposition
Stahl-Zentrum69 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
Is the lifetime-counting really state of the art?
Standard Average
Life Time, Heats 123 15
Contact Time with Steel [min] 12.800 1.600
DeviationAverage
[ ]
Time without Steel [min] 10.200 2.500
Heats/Day 6 1
Operation Days 21 3Operation Days 21 3
Bubbling:
Tapping [min] 580 70
Secondary Metallurgy [min] 2.300 320
Lance [min] 90 50
n= 53; Ladle Campaigns 2006 Feb.- August
Stahl-Zentrum70 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
; p g g
![Page 37: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/37.jpg)
Purge Plug Checking DeviceTests:1 Leckagen Detektion
Alarmierung
1. Leckagen Detektion2. Gasdurchgang Spüler Nm³/h3. O2 - Spüler freibrennen
Meß- u. RegeltechnikBedienpult
N2PC HMI
PreßluftPC HMI
Server
Standardized process and documentation!
Stahl-Zentrum71 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: R. Ehrengruber, Excellence in inert gas control systems for the steel Industry, ECCC Graz
Video
Plug Cleaning „washing“
Stahl-Zentrum72 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
![Page 38: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/38.jpg)
Gas Coupling – a safety issue!
Stahl-Zentrum73 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: MTAG Technology; Product Folder, own photos
Control Ladle Purging
Link Video
Stahl-Zentrum74 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: A. Gantner, VDEh Seminar Sekundärmetallurgie; Metallurgie des Pfannofens , 24.10.2012
![Page 39: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/39.jpg)
Steel plant and ladle logistic (1/2)
Scheduling without a logistic model is not possible!
Stahl-Zentrum75 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Steel plant and ladle logistic (2/2)
Scheduling without a logistic model is not possible!
Stahl-Zentrum76 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Scheduling without a logistic model is not possible!
![Page 40: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/40.jpg)
Ladle Logistics – Temperature Distribution
T= 60 min
17’ 33’ 50’
Stahl-Zentrum77 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: voestalpine Stahl GmbH
HKM - Gantt diagram as production planning tool
Stahl-Zentrum78 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
![Page 41: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/41.jpg)
HKM - Ladle disposition
Stahl-Zentrum79 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
HKM - Plant overview
Stahl-Zentrum80 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
![Page 42: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/42.jpg)
Ladle Logistics versus Bottom Stirring
6 6 6 6 6 6 6 6 6 6 6 6 6 6 6 6 6 6 6 66 6 6 6 6 6 6 6 6 6 6 6 6 6 6 6 6 6 6 6
26.0
2.20
0
27.0
2.20
0
28.0
2.20
0
01.0
3.20
0
02.0
3.20
0
03.0
3.20
0
04.0
3.20
0
05.0
3.20
0
06.0
3.20
0
07.0
3.20
0
08.0
3.20
0
09.0
3.20
0
10.0
3.20
0
11.0
3.20
0
12.0
3.20
0
13.0
3.20
0
14.0
3.20
0
15.0
3.20
0
16.0
3.20
0
17.0
3.20
0
6,0 5,9 6,0 5,3 5,1 6,9 6,3 5,3 5,9 5,8 6,1 2,5 3,4 3,6 3,8 3,5 5,8 5,8 6,6 6,4Heats/ Ladle
26.0
2.20
0
27.0
2.20
0
28.0
2.20
0
01.0
3.20
0
02.0
3.20
0
03.0
3.20
0
04.0
3.20
0
05.0
3.20
0
06.0
3.20
0
07.0
3.20
0
08.0
3.20
0
09.0
3.20
0
10.0
3.20
0
11.0
3.20
0
12.0
3.20
0
13.0
3.20
0
14.0
3.20
0
15.0
3.20
0
16.0
3.20
0
17.0
3.20
0
6,0 5,9 6,0 5,3 5,1 6,9 6,3 5,3 5,9 5,8 6,1 2,5 3,4 3,6 3,8 3,5 5,8 5,8 6,6 6,4Heats/ Ladle
16 16 16 16 15 14 15 15 15 16 15 13 14 15 14 12 15 14 14 15
96 95 96 85 77 96 94 80 88 93 92 33 48 54 53 42 87 81 93 96
10 8 1 14 13 11 10 11 2 2 11 9 2 8 1 13 4% L B bbli 1 '
Heats/ Day
Number of Ladles/ Day 16 16 16 16 15 14 15 15 15 16 15 13 14 15 14 12 15 14 14 15
96 95 96 85 77 96 94 80 88 93 92 33 48 54 53 42 87 81 93 96
10 8 1 14 13 11 10 11 2 2 11 9 2 8 1 13 4% L B bbli 1 '
Heats/ Day
Number of Ladles/ Day
7 10 8 24 1 7 14 13 11 7 10 11 36 2 23 2 11 9 29 2 8 15 13 41 LF1 Problem with the Bubbling System!2 Reduced Production!
% Lance Bubbling > 1 ' 7 10 8 24 1 7 14 13 11 7 10 11 36 2 23 2 11 9 29 2 8 15 13 41 LF1 Problem with the Bubbling System!2 Reduced Production!
% Lance Bubbling > 1 '
Stahl-Zentrum81 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: voestalpine Stahl GmbH
Ladle Refractories Overview
Ladle wear lining
Bricks MonolithicsBricks
Non-basic Basic
Monolithics
Non-basic Basic
Burned Unburned Burned Unburned
Phosphate-bonded
Carbon -bonded
Burneddoloma
Magnesia-chrome
Doloma-carbon
Magnesia-carbon
Stahl-Zentrum82 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: T. Molinari et al, Optimized Refractory Solutions for High Performance Ladles and RH Degarssers, BHM Heft 5 (2003)
![Page 43: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/43.jpg)
Overview of Ladle Refractory Working LiningsType Advantage Disadvantage Application area
Magnesia-Carbon High refractoriness L i i idi i hBottomSid llMagnesia Carbon
(MgO-C)High refractorinessResistant: basic slags + infiltration Low resistance in oxidising atmospheres Sidewall
Slagline
Alumina-Magnesia-Carbon-Spinell(AMC)
Abrasion resistanceIrreversible thermal expansion
Lower chemical resistance (silica slags)
Bottom Impact areaSidewall(AMC)
Monolitic(Alumina-mixes)
Fast installationLess break out materialC-free lining
Longer heating timeEquipment investment
BottomSidewall
D l it C b Infiltration resistant to basic, low Danger of Hydration BottomSid llDolomite-Carbon Infiltration resistant to basic, low
FeO slags; Low structural spallingDanger of HydrationLow resistance: alumina slags Sidewall
Slagline
Burnt Alumina-Spinel C-free lining Lower chemical resistance Bottom
Sidewall
Corrosion resistant at slag change Infiltration and C2S Disintegration BottomBurnt Magnesia-Chromite
Corrosion resistant at slag changeHigh erosion resistance35%-100% VOD heats
gLow resistance against temperature changes (spalling)Lower resistance against reducing slags
SidewallSlagline
Burnt DolomaLower infiltrationRecistance against reducing slags20% 0% O
Low resistance against temperature changes (spalling)
BottomSidewallS
Stahl-Zentrum83 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
20%-70% VOD heats Lower corrosion resistance atslag change Slagline
Source: RHI- AG; Product Management Linings Steel (2016)
Layered Lining of the Ladle
I l tiInsulation
Pre- insulation
Safety lining
Backfilling
Wear lining
Stahl-Zentrum84 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: RHI- AG; Product Management Linings Steel (2016)
![Page 44: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/44.jpg)
Common Wear Linings for Steel Ladles
Slag line:Slag line:Slag line: MgO-C, 10-15% C Dolomite-C
Side wall and bottom:
Slag line: MgO-C, 10-15% C Dolomite-C
Side wall and bottom:S de a a d botto MgO-C, 5-10%C Dolomite-C
(Bauxite)Al2O3 MgO C bricks (AMC)
S de a a d botto MgO-C, 5-10%C Dolomite-C
(Bauxite)Al2O3 MgO C bricks (AMC) Al2O3-MgO-C-bricks (AMC)
Monolithic Burned Alumina-Spinell bricks
Impact area:
Al2O3-MgO-C-bricks (AMC) Monolithic Burned Alumina-Spinell bricks
Impact area:Impact area: Al2O3-MgO-C-bricks (AMC) MgO-C, 5%C, fused Magnesia
Impact area: Al2O3-MgO-C-bricks (AMC) MgO-C, 5%C, fused Magnesia
Stahl-Zentrum85 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: RHI- AG; Product Management Linings Steel (2016)
Ladle Refractory Solutions
Carbon and resin bonded wear lining bricks Carbon and resin bonded wear lining bricks Magnesia, Alumina-Magnesia, Doloma
Burnt wear lining bricks based on: Magnesia-Chromite, Alumina-Spinel, Doloma
Monolithic wear lining Low-cement, self- flowing, oxycarbide
Ramming, casting and gunning mixes Alumina, Magnesia, Doloma (ramming only)
Purge plugs Porous, Slot, Star, Labyrinth, Segment, Hybrid
Permanent lining and Insulation
Prefabs
Stahl-Zentrum86 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: RHI- AG; Product Management Linings Steel (2016)
![Page 45: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/45.jpg)
Wall:
HKM - Ladle Permanent Lining Configuration
30mm steel shell
20mm vermiculite board
90 A d l it 90mm Andalusite
Slag zone: Magnesia-spinel
32mm burnt Magnesia32mm burnt Magnesia
Bottom: 54mm steel shell
30mm insulating alumina castable
90mm high alumina castable
Stahl-Zentrum87 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
32mm burnt MagnesiaSource: H. Schröter HKM (2016)
HKM - Ladle Thermal Conductivity Calculation
Stahl-Zentrum88 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
![Page 46: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/46.jpg)
Monolithic bottom and sidewall, MgO-C bricks slag line
Stahl-Zentrum89 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: Viertauer, Exenberger 2003 14th IAS Steelmaking Conference San Nicolas, Argentina; Efficient Ladle Management at voestalpine Stahl GmbH
Metallurgical results between different lining concepts
ULC grades are produced at an RH degasser!
Stahl-Zentrum90 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: R. Exenberger, VDEh Seminar Steel Ladle Lining, Saarbrücken/ Germany, Sept. 2014
ULC- grades are produced at an RH- degasser!
![Page 47: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/47.jpg)
VD- treatment and decarburization
Stahl-Zentrum91 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Lachmund, VDEh Seminar Steel Ladle Lining, Luly 2014
ULC- grades are produced at an VD- degasser!
280t capacity
HKM - Steel ladle key data
125t tara (relined)
40t wear lining
Vac / Al-thermic heating limit = 0-72 heats Vac. / Al-thermic heating limit = 0-72 heats
Av. wear = 72 heats
Bottom stirring (2x purging plug; Paul-W th l t h)Wurth-clutch)
CS100 Slide gate
Stahl-Zentrum92 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
![Page 48: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/48.jpg)
Part Quality Format97 98%M O Hi h P it
HKM - Steel Ladle Refractories
Slagzone 97-98%MgO High PurityFused Magnesite / >9%C 5P
Wall 96-97%MgO Fused Magnesite +Sintered Magnesite / >9%C 3P
Reinforced wall (Tapping)
97%MgO Fused Magnesite +Sintered Magnesite LC / 5%C
92%Al2O3 (Tab) / 6%MgO / 6%C
4P/5P
Tapping-pad 81,5-92%Al2O3 (Fused Alumina/Tab)/ 5-7,5%MgO / 4-7,3%C (Resin) 350mm77-86%Al2O3 (Bauxite)/ 6-9%MgO
Bottom77-86%Al2O3 (Bauxite)/ 6-9%MgO/ 5-7%C (Resin)94%MgO Sintered Magnesite/ 4%C (Resin)
250mm
Stahl-Zentrum93 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Limit Max 71 heats for VD (Ladle top and slag line)Source: H. Schröter HKM (2016)
Benchmark life time and refractory consumption
StandardA[kg/t] mm/Heat
Impact Area 0,03 ~1,80Bottom 0,18 ~0,8Wall 0,25 ~0,4
Life Time, Heats 123 15
Contact Time with Steel [min] 12.800 1.600
Time without Steel [min] 10 200 2 500
Standard DeviationAverage
Slag Line 0,37 (0,19*) ~0,65
Gunning (Slag Area) ~0,09Bottom (Permanent Lining) ~0,01Wall (Permanent Lining) ~0,04
Time without Steel [min] 10.200 2.500
Heats/Day 6 1
Operation Days 21 3
Bubbling:
Slag Line (Permanent Lining) ~0,03
Impact Area: AMC; Bottom and Wall: Castable; Slag Line: MgO-C Bricks
Source: SAP consuption [kg] refractory; FJ 2006
* [kg] rest material weight / number of heats / heat weight
Tapping [min] 580 70
Secondary Metallurgy [min] 2.300 320
Lance [min] 90 50
n= 53; Ladle Campaigns 2006 Feb.- August
Stahl-Zentrum94 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: A. Viertauer, 3rd int. Symposium Steel Ladle Lining; Efficient Laldle Management at voestalpine Linz, Ijmoiden NL2004
![Page 49: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/49.jpg)
Ladle empty Contact time
HKM - Ladle empty and steel contact time since 2003
Now 3 - 4 heats / day
Stahl-Zentrum95 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
ySource: H. Schröter HKM (2016)
HKM - Ladle Performance Figures
Heats/day 3-4
Vacuumdegassing 55-70%
Al th i H ti 5% Alumothermic Heating 5%
Ladle Heating Stands 7 (1100°C)Ladle Heating Stands 7 (1100 C)
Stahl-Zentrum96 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
![Page 50: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/50.jpg)
HKM - Tapping Temperature 2004 - 2015
Stahl-Zentrum97 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
Visible inspection of refractory
HKM - Ladle Servicing
p y
Gunning of the top, well block, purging plugs
Inspection and replacement of slide gate plates, nozzles & purging plugs
Check of AMEPA system
Check of purging system
Heating of ladles
Cleaning
Stahl-Zentrum98 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
![Page 51: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/51.jpg)
HKM - Ladle Service
Cooling 3 shifts
Breakout and lining (work lining) 7 shifts
M i t 1 2 hift Maintenance 1-2 shifts
Preheating (1100°C Oxygen 300°C-800°C) 24hPreheating (1100 C, Oxygen 300 C 800 C) 24h
Stahl-Zentrum99 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
Evaluation of action fields
HKM - Ladle Remaining Wear Lining Thickness Report
Stahl-Zentrum100 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
![Page 52: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/52.jpg)
Bottom Construction
Continuous: Stable construction Bottom change not possible Correct bottom brickwork in order to
get a flat basis for the side wallget a flat basis for the side wall
Inserted: Bottom change possible Easier installation Bottom joint is a weak point Therefore choose a good ramming Therefore choose a good ramming
mass and work carefully
Stahl-Zentrum101 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: RHI- AG; Product Management Linings Steel (2016)
P-Shapes (Side Arch Bricks)
Brick height 250mm, Width approx. 100mm
High brick weight Example: 4P8 ~ appr. 14kg
Less Joints Less Joints Specific joints 14m/m²
Installation Layer per layer one or two cuts per layer required Layer per layer - one or two cuts per layer required High brick height leads to: Fast installation High mechanical stabilityg y
Problems with steps and open joints in conical ladles
Stahl-Zentrum102 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: RHI- AG; Product Management Linings Steel (2016)
![Page 53: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/53.jpg)
Problems with P-Shapes in Conical Ladles
Installation following the ladle conus:Installation following the ladle conus:opening of „V“-joints at the upper end of the layer
Installation vertical:steps with the disadvantage of:loss of effective brick length increased spalling
Solution: in conical ladles use bricks with a height of 100mm (Mini Keys or SU-shapes) only!
Stahl-Zentrum103 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: RHI- AG; Product Management Linings Steel (2016)
Mini Keys (MK)Brick height 100mm, Width 150mm in the middle
Easy to handle due to less brick weight Example: MK7/8 ~ appr. 8kg
Many joints Specific joints 18,7m/m2
33% th P h 33% more than P-shapes
Installation Layer per layer - one or two cuts per layer requiredLayer per layer one or two cuts per layer required Spiral lining also possible, but not in common use
Suitable for conical ladles
Stahl-Zentrum104 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: RHI- AG; Product Management Linings Steel (2016)
![Page 54: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/54.jpg)
Lining with P- and MK-Shapes: The Closing BrickThe closing bricks shall: Not be in the trunnion area
Not be directly above purge plug andslide gate
From one ring to the next not be directly above each other.
Fit the remaining gap tightly, which means g g p g y,that it has to be inserted with a rubber hammer (inserting only by hand is not enough)
If the remaining gap is smaller than 50mm two closing bricks have to be cut and inserted with at least 2 uncut bricks between them
Stahl-Zentrum105 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
between themSource: RHI- AG; Product Management Linings Steel (2016)
Sidewall Construction - Find the Mistakes!
Stahl-Zentrum106 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: RHI- AG; Product Management Linings Steel (2016)
![Page 55: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/55.jpg)
Lining with P- and MK-Shapes: The keys
Mix of keys 1:1 Mix of keys >3:1 Uniform gap between wear and
permanent lining
Small deviations of key no bl
Strongly varying gap between wear and permanent lining
Small deviation of key can make l dl “ li bl ”
Stahl-Zentrum107 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
problem ladle “un- line able”Source: RHI- AG; Product Management Linings Steel (2016)
Semi Universal (SU)Brick height 100mm, Width 210mm on the cold side
Brick weight Example: SU745 ~ appr. 10,5kg
Joints Specific joints 17,4m/m² 25% more than P-shapes
Installation Especially developed for spiral lining Fast installation Only one shape per ladle Starter set or ramp necessary (cast rammed) Starter set or ramp necessary (cast, rammed) Lower mechanical stability – no closed rings Layer by layer also possible, but not in
common use
Stahl-Zentrum108 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Suitable for conical ladlesSource: RHI- AG; Product Management Linings Steel (2016)
![Page 56: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/56.jpg)
Permanent Lining Bricks
SL ShR t l h NF ShSL ShapesRectangular shapes NF Shapes
Bottom, Insulating bricks
Wedged SL-Shapes are preferred in the sidewall for better safety
Safety lining side wall
Stahl-Zentrum109 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: RHI- AG; Product Management Linings Steel (2016)
Monolithic Safety Lining
Two possibilities:1.) Casting behind the brick layers. Depending on the material of the monolithic safety lining and the shape of
Insulation
material of the monolithic safety lining and the shape of the wear lining bricks, application every 1-7 layers
2.) Casting with a template like the monolithic steel Monolithic
safetyladle lining is also a possibility (Not for dry monolithic material)
safety lining
Wear lining
Stahl-Zentrum110 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: RHI- AG; Product Management Linings Steel (2016)
![Page 57: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/57.jpg)
Template for monolithic ladleSelf flowing mixes Template with reinforcements in
Thixotrophic mixes Template with electric vibrators Template with reinforcements in
Impact and purge plug area Template with electric vibrators
Stahl-Zentrum111 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: RHI- AG; Product Management Linings Steel (2016)
Demands on the Permanent Lining of Ladles
Emergency operation: Permanent lining has to withstand at least 1 heat or moreEmergency operation: Permanent lining has to withstand at least 1 heat or more
Permanent linear change > 0% at 1600°C
Thermal conductivity not too high…..y g
Sufficient strength
Sufficient refractoriness
Resistance to carbon bursting
Stahl-Zentrum112 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: RHI- AG; Product Management Linings Steel (2016)
![Page 58: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/58.jpg)
Safety lining solutions
P d t t Thermal Cold hi
Thermal h k Emergency Application Danger of
bProduct type Thermal conductivity crushing
strengthshock
resistance
Emergency properties
Application area carbon
bursting
Burnt Bauxite medium high very high medium Bottom/Sidewall Yes
Burnt Mullite Low medium high very high medium Bottom LowBurnt Mullite Low-medium high very high medium /Sidewall Low
Magnesia-Chromite medium medium high very high VOD-ladles Yes
Burnt Magnesia high high low high Slagzone No
Burnt Magnesia-Spinel high high Medium-high high Slagzone No
Dry monolithic material medium low high medium universal No
Burnt Fireclay low medium high very low not advised Yes
Magnesia Carbon very high low medium very high not advised No
Stahl-Zentrum113 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: RHI- AG; Product Management Linings Steel (2016)
Types of Ladle Insulation
Product type Thermal conductivity
Cold crushing strength
Maximum application temperature
Application area
Insulating fired brick low very low 1400°C PreinsulationInsulating fired brick low very low 1400 C Preinsulation
Ceramic fiber very low extremely low 1250°C Insulation
Vermiculite low ok 1100°C Insulation
Microporous Insulation extremely low nonexistent 1000°C Not advised
Stahl-Zentrum114 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: RHI- AG; Product Management Linings Steel (2016)
![Page 59: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/59.jpg)
Thermal conductivity through a ladle side wall
sula
tion
tion
shel
l
ckfil
ling
Pre-
in
Wear liningPermanent
lining Insu
lat
Stee
l
Bac
Stahl-Zentrum115 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: RHI- AG; Product Management Linings Steel (2016)
Drying and Heating
Stahl-Zentrum116 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: R. Exenberger, VDEh Seminar Steel Ladle Lining, Saarbrücken/ Germany, Sept. 2014
![Page 60: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/60.jpg)
HKM - Ladle Preheating
Stahl-Zentrum117 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
MgO – C Bricks and Oxidation
burnt-outCarbon binding matrix
intactCarbon binding matrixCarbon binding matrix Carbon binding matrix
Stahl-Zentrum118 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Reason: Oxidation !
![Page 61: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/61.jpg)
HKM - Ladle Preheating - decarburization
Stahl-Zentrum119 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
Wear Influence by process
MetallurgicalMetallurgical Reactions with steel / slag / fluxes / alloying materials Reactions with atmosphere / vacuum …..
Process Electric arc radiation Erosion caused of purging / flow / tapping ….
Logistics Contact time full / empty / transport Thermal stress Thermal stress ….
Stahl-Zentrum120 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
![Page 62: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/62.jpg)
ChemicWear influence – Refractory material properties
Infiltration Reduction Oxidation Evaporate
St t h i Structure changing
Thermic Expansionp Treatment time- contact time Thermal stress and shock Structure changing
M h iMechanic Erosion Transport Cleaning
Stahl-Zentrum121 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Function: 1 R f t i l l
Refractory Lab
1. Reference material samples
2. Analysis and physical properties of reference material, sewed plates
3. „Fingerprint“ by xrd of reference material
4. 4x/a sampling, retained samples, weight, dimensional accuracy, bulkweightweight
5. Possibility to determine bulk density,waterabsorption, open porosity,linear shrinkage (drying @110°C),sieve analysis
Stahl-Zentrum122 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
![Page 63: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/63.jpg)
Refractory Lab: Fingerprint by XRD
PANalytical Cubix3
Röntgenbeugung, X-ray diffraction (XRD)
Stahl-Zentrum123 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Analyse der mineralogischen PhasenSource: P. Peternel SZMF, K. Walter, HKM 2016
Refractory Lab: Fingerprint by XRD
1. Average sampling
2. Grind the granulated material < 90 µm
3 Press the sample for XRD measurement3. Press the sample for XRD measurement
4. Start XRD measurement with PANalytical Cubix3
5. Interpretation of the diffractogram
Stahl-Zentrum124 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: P. Peternel SZMF, K. Walter, HKM 2016
![Page 64: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/64.jpg)
Refractory Lab: Fingerprint by XRD
Example: Mould Flux
Stahl-Zentrum125 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: P. Peternel SZMF, K. Walter, HKM 2016
Test method: Induction Furnace Slag TestTest method: Induction Furnace Slag Test
HKM - Lab test for permanent lining
Test method: Induction Furnace Slag Test
Temperature: 1700°CHolding time: 4 hours
Test method: Induction Furnace Slag Test
Temperature: 1700°CHolding time: 4 hoursMelt: Steel CrMnSi 6-4Slag: CA-richAtmosphere: Air
Melt: Steel CrMnSi 6-4Slag: CA-richAtmosphere: Air
Slag Composition: weight % Component52 CaO30 Al2O37 SiO2
Slag Composition: weight % Component52 CaO30 Al2O37 SiO27 SiO26 MgO5 CaF2
7 SiO26 MgO5 CaF2
Stahl-Zentrum126 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
![Page 65: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/65.jpg)
Wall
HKM - Ladle Permanent Lining Configuration
Main Component:
Alumina enriched Andalusite
Wear Rate (CA-slag): 19 mm/h
Slag zoneMain Component:
Fused Magnesite + Bauxite
Wear Rate (CA-slag): 1 mm/h
Stahl-Zentrum127 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
Benefits:
Long term evaluation of material properties (e g nut feather system worn form 1x reclamation
Refractory Lab
Long term evaluation of material properties (e.g. nut feather system, worn form, 1x reclamation refractory supplier)
Quick test for material confiusion by comparison of sewed plates (2x reclamations ref. supplier, 1x contractor))
Detection of inner cracks (1x reclamation ref. supplier) and damaged edges (1x prohibition of delivery)
Quick Test for water content linear drying shrinkage (1x reclamation ref supplier) Quick Test for water content, linear drying shrinkage (1x reclamation ref. supplier)
Detection of raw material substitution (1x ref. supplier liquidation before reclamation)
Gaining knowledge of the employees
Open and honest discussion with the supplier and contractor
Delivery of less flawed material
Stahl-Zentrum128 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Gaining safety of the processSource: H. Schröter HKM (2016)
![Page 66: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/66.jpg)
New and used Ladle
Stahl-Zentrum129 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: A. Viertauer, VDEh Steel Academy, Refractory Technology Steel Ladle Lining , Efficient Ladle Management at voestalpine Stahl, Linz 2006
Laser Mirror ScannerFixed Installation „Moving Device“
Stahl-Zentrum130 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source photos: left voestalpine Stahl GmbH , right: Ferrotron
Source: A. Viertauer, VDEh Steel Academy, Refractory Technology Steel Ladle Lining , Efficient Ladle Management at voestalpine Stahl, Linz 2006
![Page 67: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/67.jpg)
Ladle Refractory – Wear MeasurementTerminal
Inclinometer
LASER MIRROR SCANNER
Stahl-Zentrum131 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM Source: voestalpine Stahl GmbH
Source: A. Viertauer, VDEh Steel Academy, Refractory Technology Steel Ladle Lining , Efficient Ladle Management at voestalpine Stahl, Linz 2006
Measurement Steps
1 2 43
Trunnion Ring Wall North Bottom Wall South
Stahl-Zentrum132 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: A. Viertauer, VDEh Steel Academy, Refractory Technology Steel Ladle Lining , Efficient Ladle Management at voestalpine Stahl, Linz 2006
![Page 68: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/68.jpg)
Laser Measurements during a campaign
New Lining
Stahl-Zentrum133 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: A. Viertauer, VDEh Steel Academy, Refractory Technology Steel Ladle Lining , Efficient Ladle Management at voestalpine Stahl, Linz 2006
Does the Laser Measurement gives us more safety?
1st The information about „remaining thickness“ is just an information!2nd Each measurement has to be checked for plausibility!3rd The area between bottom and wall is not measured, it is calculated! There are two coordinate systems one for the bottom – one for the wall!4th Joints and small holes can not be detected! The reason is the density of the measuring points and the mathematical inter- and extrapolation!
Stahl-Zentrum134 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
measuring points and the mathematical inter and extrapolation!Source: A. Viertauer, VDEh Steel Academy, Refractory Technology Steel Ladle Lining , Efficient Ladle Management at voestalpine Stahl, Linz 2006
![Page 69: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/69.jpg)
Hot Spot Detection (1/2)
Stahl-Zentrum135 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: Paper AIS Tech 2006 Cleveland, May 2006; SIEMENS- VAI
Hot Spot Detection at the LF (2/2)
Stahl-Zentrum136 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: Flyer Hot Spot Detection, Agellis Group, 2014
![Page 70: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/70.jpg)
HKM - Thermo Scan Steel Shell Ladle
Video
Stahl-Zentrum137 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
Cobble stoning – deep horizontal and vertical joints
Stahl-Zentrum138 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: 2007 VDEh Steel Academy Refractory Technology II, Ladle Metallurgical Treatments & Refractory Stress for a Steel Teeming Ladle
![Page 71: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/71.jpg)
Ladle Gunning – especially slag line and lip ring
Stahl-Zentrum139 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source Photos: RHI, voestalpine Linz, Bhushan, JSW- T
Lipring
Function: Vertical Fixing of the Lining
Problems: Forces from slag skull removal
Sl d t l l hi d fl Slag and steel splashing and overflow Scaling Installation to complicated Bending upwards by thermal expansion of the
li ilining
Results: Loss of bricks
O f S f Opening of horizontal joints Steel infiltration Bended Lipring No vertical fixing
Stahl-Zentrum140 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: Product Management RHI
![Page 72: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/72.jpg)
Lipring – Classic InstallationsShort Lipring, unprotected, bad clamping,… Reinforced on the outside, unprotected
Reinforced on the outside, quickly exchangeable, unprotected
Inclined lipring, protected ,expensive closing brick
Stahl-Zentrum141 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: Product Management RHI
LipringUntil 1/2-2/3 of wear-lining brick length!
Optimal solution: High mechanical stability g High mechanical stability Good clamping of the lining Easy and fast installation High thermal stability
Ramming/Casting
High thermal stability High lifetime => less maintenance Allowance for the thermal expansion of the
liningg Enough free board
A tailor made solution for each PermanentLining and Insulation
Wear Lining
A tailor made solution for each customer has to be found
Stahl-Zentrum142 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: Product Management RHI
![Page 73: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/73.jpg)
Prewear Impact Area – two solutions
Fotos: voestalpine Stahl GmbH
Stahl-Zentrum143 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: 2007 VDEh Steel Academy Refractory Technology II, Ladle Metallurgical Treatments & Refractory Stress for a Steel Teeming Ladle
Spalling (1/3)
Drying Simulation:Shrinking hot side 0,275 mm and cold side 0,199 mm
Stahl-Zentrum144 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: CD Laboratory Leoben, Photos: voestalpine Linz
![Page 74: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/74.jpg)
Spalling (2/3)Ladle crane transport Tension- and compression load
Stahl-Zentrum145 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: CD Laboratory Leoben, Photo: voestalpine Linz
Spalling of resin bonded material (3/3)
Stahl-Zentrum146 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
![Page 75: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/75.jpg)
HKM - Bricks moved out – shrinking 1/2
Ladle was laying horizontal and getting cold!
Stahl-Zentrum147 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
HKM - Bricks moved out – shrinking 2/2
Bricks move out when ladle laying while cold
Stahl-Zentrum148 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
![Page 76: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/76.jpg)
Horror Cabinet
Stahl-Zentrum149 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Ladle 66, age 60, breakout 0°, joint layer 15/16
HKM - Ladle Break out – false repair
joint layer 15/16
Stahl-Zentrum150 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
![Page 77: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/77.jpg)
HKM - Ladle Break out – false repair
After lining noAfter lining no open joints
Stahl-Zentrum151 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
HKM - Ladle false repair
Steel infiltrationinfiltration in joints layers: 15/1615/16, 16/17, 17/18
Stahl-Zentrum152 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
![Page 78: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/78.jpg)
HKM - Ladle false repair
Monolithic skimmer lost (view on bricks)
“Hotrepair” with Olivine / Sintermagnesia gunning refractory in the age 46
Stahl-Zentrum153 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
HKM - Steel Ladle
Stahl-Zentrum154 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
![Page 79: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/79.jpg)
HKM - Ladle wrong ladled material
Spillinglayer 3, 0°,1x brick
Stahl-Zentrum155 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
HKM - Ladle wrong labeled material
Stahl-Zentrum156 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
![Page 80: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/80.jpg)
Labeling in
HKM - Ladle wrong labeled material
Labeling in brickworks – white line
Stahl-Zentrum157 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
HKM - Ladle wrong labeled material
Materialcompletelylabled –mistake bysupplier
Stahl-Zentrum158 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
supplierSource: H. Schröter HKM (2016)
![Page 81: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/81.jpg)
HKM - Ladle material confusing
Only 4P/4-f tformatsaffected
Stahl-Zentrum159 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
Horror Cabinet – explosion of wrong material
HKM - Ladle Servicing
ULC castable exploded throughthrough heating up
porosity too p ylow!
Stahl-Zentrum160 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
![Page 82: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/82.jpg)
Problem Area Slag Line – Constructive Solutions
Stahl-Zentrum161 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: 2007 VDEh Steel Academy Refractory Technology II, Ladle Metallurgical Tratments & Refractory Stress for a Steel Teeming Ladle
Break – Through Ladle Slag Line
Fe SiO2 Mn CaO MgO Al2O3 P2O5 Cr2O3 K2O TiO2
Slag composition after the break through:
Does the permanent lining have emergency running properties?
0,52 4,94 0,07 50,48 15,14 27,75 0,013 0,01 0,001 0,154
Stahl-Zentrum162 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
running properties?
Source: 2007 VDEh Steel Academy Refractory Technology II, Ladle Metallurgical Treatments & Refractory Stress for a Steel Teeming Ladle
![Page 83: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/83.jpg)
Prewear Wall - Bottom
Stahl-Zentrum163 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: 2007 VDEh Steel Academy Refractory Technology II, Ladle Metallurgical Treatments & Refractory Stress for a Steel Teeming Ladle
Damaged Plugs
too intensive O2 cleaning too high line pressure 2 g
(>> 20 bar)
Stahl-Zentrum164 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: RHI
![Page 84: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/84.jpg)
Blocked purging slits – possible Rasons?Very thin
carbon layercarbon layer
deep steel penetrationpenetration
Stahl-Zentrum165 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: 2013 04 VDEh Steel Academy Refractory Technology II, Ladle Metallurgical Treatments & Refractory Stress for a Steel Teeming Ladle
Stirring is not possible – what could be the reason?Possible reasons are: Ladle logisticLadle logistic.. “Water pump effect” Quick disconnecting – negative flow (back attack) Contaminated purging gas Purging Gas Supply
Gas Leakage
Deep steel penetration in the purging slots!
Liquid Steel
Stahl-Zentrum166 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Liquid Steel
Source: 2013 04 VDEh Steel Academy Refractory Technology II, Ladle Metallurgical Treatments & Refractory Stress for a Steel Teeming Ladle
![Page 85: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/85.jpg)
Stirring was not possible – what could be the reason?
Al closed theAl closed the purging slots !
Stahl-Zentrum167 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: 2013 04 VDEh Steel Academy Refractory Technology II, Ladle Metallurgical Treatments & Refractory Stress for a Steel Teeming Ladle
HKM - Ladle slide gate break out
Plate age 2; 138’ casting;Ca = 7 / 13 Nut in slide gate
Stahl-Zentrum168 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
![Page 86: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/86.jpg)
Horror Cabinet – purging plug breakout
Purging plug breakout
HKM - Ladle Servicing
Purging plug breakout (280 t steel in the VD-tank)
Stahl-Zentrum169 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
HKM - Ladle purge plug break out
Stahl-Zentrum170 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
![Page 87: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/87.jpg)
HKM - Ladle Purge Plug break out
DE-samples
red = purging plug from breakout ladle
black = new purging plug p g g p g(chemistry ok)
Stahl-Zentrum171 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
Limiting factors of wear: deskullingDeskulling + ladle design
Stahl-Zentrum172 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
![Page 88: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/88.jpg)
Limiting factors of wear: steel bath / slag level (tapping weight)
Premature wear of Alumina-based refractories byrefractories bylime saturated slag
Stahl-Zentrum173 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
Limiting factors of wear: ladle lifetime
Wearmechanism Heating up tapping slag pressure Heat
transitionTime ladle empty purging
Avoidable Decarburizationby Lambda >1,
Premature wearby tapping beam
Premature wearby aggressive
High wear ratesby
Decarburizationby long times
Wear by badposition of plugs
or long time between heatingup and 1st melt
out of position slags (Basicitylow esp. incombination withCaF2, no MgOadding, SiO2)
(over)insulation ladle empty (hotstate)
Explosions bywater overdosis
Premature wearby high amount
Hightemparaturewater overdosis,
wrong material (dense), toosteeptemperaturecurve
by high amountof BOF slag in SEM
temparaturelosses due toshort or no ladleheating duringtime ladle empty
Cracks by toosteeptemperaturecurve
Not avoidable Decarburization wear by tapping Wear by slag Reduction of wear by high Decarburization Wear by bathNot avoidable Decarburizationby false air, coldface
wear by tappingbeam in rightposition
Wear by slaginfiltration
Reduction ofMgO by Al, C under vacuum
wear by high bordertemperatures
Decarburizationin time ladlemaintenance, slag droppingbetween melts
Wear by bathmoving whilepurging
Wear by hightappingt t
Wear by slagsolving MgO, C O Al2O3 t
Temperatureshock due toT t
Stahl-Zentrum174 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
temperatures CaO, Al2O3 etc. during forming
Temparaturedrop while empty
Source: H. Schröter HKM (2016)
![Page 89: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/89.jpg)
Limiting factors of wear: ladle lifetime
Wearmechanism deskulling
Electrothermic / alumothermic heating
Steel bath
Avoidable Damage ofAvoidable Damage ofrefractory by latedeskulling
Damage ofrefractory by baddeskullingg
Not avoidable Damage ofrefractory by
Wear by hot spot(radiation heat
Solution ofcarbon in liquid
„toothing“ of steelwith refractory
impact, lowviscosity of slag)
steel
Wear by low slagbasicity in caseof Al-thermicheating
Stahl-Zentrum175 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
Frequency of mistakesSteel Plant Operations
Stahl-Zentrum176 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Lining InstallationRefractoriesSource: H. Schröter HKM (2016)
![Page 90: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/90.jpg)
Frequency of mistakes - Refractories
Wrong labelingWrong labeling
Insufficent mixing (mixing time too short / long, esp. fine material in low values spread worse, demixing by vibration in silo/-vehicle)
False stored / overlaid material False stored / overlaid material(binder reacted with moisture, material damaged by frost)
Dimensional accuracy insufficient (Form “washed out”, warpage through drying / burning)y g g)
Foreign bodies in material(cuttings, abrasion dust, bolts, pieces of conveyor belts, etc.)
Wrong components in recipe (Mistakes in program, dirty production line, leak g p p ( p g y pbunkers, rests from former load in silovehicle, mistakes of staff, weighing mistakes, wrong bunkercontent, insufficient raw material entrance inspection, purpose, etc.)
Stahl-Zentrum177 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
Wrong amount in recipe (insufficient weighing exhausting of fine
Frequency of mistakes - Refractories
Wrong amount in recipe (insufficient weighing, exhausting of fine material)
Damaged material (outbursts on edges, pressing layers, over pressing, damaged form, etc.)g , )
Insufficient pretreatment (material not dried, wrong temper-/ burning temperature curve, insufficient impregnation)
Wrong choose of materialWrong choose of material
Stahl-Zentrum178 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
![Page 91: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/91.jpg)
Frequency of failures – Lining Installation
Too much / less water / binder (“with less water the mass is notToo much / less water / binder ( with less water the mass is not flowing”)
Wrong adjusted gunning machine (pressure, watervalve)
I t l Impure tools (plate mixer is running for days, insufficient cleaning of mixer between mixes)
Drying time too short (spilling)
Heating curve: too steep (spilling), too long (decarburization), too short (spilling in service)
Confusion of materialConfusion of material
Insufficient joints (too wide, throughout joints)
Stahl-Zentrum179 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
Frequency of failures – Lining Installation
Damage through lining (metal hammer)
Wrong tools (gunning of a casting material, dents in the pattern, worn feeler )gauage)
Stahl-Zentrum180 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
![Page 92: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/92.jpg)
Frequency of mistakes – Steel Plant Operations
Manipulation by telescope digger (damage of lining through deskulling,, p y p gg ( g g g g,,pushing of well block and purging plug)
Touch down of the ladle (damage of purging pipework or PWK, accidental opening of slide gate, warpage / damage of slide gate housing / -linkage)
Misjudgment and negligence (early drop at high residual thickness, no detection of too low residual thickness or gap between slide gate plates)
Flawed repairs (wrong material, too much / few water / mortar, deficient setting of purge plugs inner nozzles slide gate plates SEN)purge plugs, inner nozzles, slide gate plates, SEN)
Deficient heat balance (“too long” parking of ladle - decarburization, cool down of ladle – opening joints, frequent heating / over boiling under vacuum)
Wrong position of tapping beam Wrong position of tapping beam (premature wear of sidewall- or bottom lining)
Chemistry of Slag (“wasting” of fluorspar in case of dry slag / low purging, too high amount of converter slag / “super blown” heats)
Stahl-Zentrum181 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: H. Schröter HKM (2016)
Outlook - Refractory Control System
Stahl-Zentrum182 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Source: P. Razza, A. Yaseen, G. Lammer, A. Rom, A. Hanna; Statistical Data Analysis for Process Improvements at Emirates Steel Adu Dhabi; AISTech (2015)
![Page 93: STEEL TEEMING LADLE: Ladle Metallurgical Treatment ...A special frame which is located on a service car or on a frame which will be settled onto the ladle transfer car 23 | 24 to 27.](https://reader030.fdocuments.in/reader030/viewer/2022012900/5e540b9bc074e07a5b5b88d3/html5/thumbnails/93.jpg)
ContentMetallurgical Tasks
Steel Production overview
Example: ULC, HIC, TRIP, TWIP
Secondary Metallurgy Tasks
Aggregates vs. Refractories
Ladle slag
Purging instrumentation
Teeming ladleTeeming ladle Lining concepts
Wear mechanism
Lab investigation
D i d h ti Drying- and heating
Laser- vs. Thermo vision Scan
Purging
„Problem areas“ and Check list
Stahl-Zentrum183 | 24 to 27. April 2016, Cologne, Refractory Technology Part II, Steel Teeming Ladle,· A. Viertauer/ RHI-AG, H. Schröter/ HKM
Outlook and Summary