ASTM D5744 Kinetic Test Method Status and...
Transcript of ASTM D5744 Kinetic Test Method Status and...
![Page 1: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/1.jpg)
ASTM D5744 Kinetic Test Method Status and Application
Minnesota DNR20th Annual BC-MEND Workshop
4 -5 December 2013
![Page 2: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/2.jpg)
ASTM D5744-13: Standard test method for laboratory weathering of solid materials using a humidity cell
• Kinetic test – Laboratory mine waste dissolution test– Mine waste drainage quality prediction
• Status– Most recent modification in 2013
• Application – Mine waste management
![Page 3: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/3.jpg)
OUTLINE
1. Mine waste characterization introduction2. ASTM D5744 development, rigor3. ASTM D5744 method description4. Kinetic test application– Reactivity– Rates of solute release
Note: Focus on waste rock
![Page 4: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/4.jpg)
(1) MINE WASTE CHARACTERIZATIONIntroduction
• Solid-phase characterization– Ore deposit type (geoenvironmental modeling)– Visual examination (drill core logging)– Chemical analysis– Metal partitioning– Mineralogical/petrological analysis– Static tests (acid and neutralization potentials)
![Page 5: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/5.jpg)
(1) MINE WASTE CHARACTERIZATIONIntroduction
Drainage quality = f(solid-phase characteristics)
• Short-term dissolution tests (soluble salts)• Kinetic tests (long-term dissolution tests) – Soluble salts, other mineral dissolution
• Geochemical modeling
![Page 6: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/6.jpg)
(2) ASTM D5744 DevelopmentWHAT?
• Detailed laboratory weathering test method Kinetic test for waste rock8 drafts from 1992-1996
• Reviewed in formal ASTM processPractitioners, industry, academia
• Rigorous ruggedness testing• Revisions 2007, 2013
![Page 7: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/7.jpg)
(2) ASTM D5744 Development Ruggedness testing
• Intralaboratory and interlaboratory testing
• 68 samples from 6 different rock types– Characterized: p. size, chemistry, mineralogy– Comparative testing for 20 -265 weeks
• Results in 111 p. research report w/method
![Page 8: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/8.jpg)
(2) ASTM D5744 DevelopmentWHAT?
Formalized, robust waste rock dissolution test method
WHY?
• Provide detailed description of protocol– Based on existing methods (Lawrence 1990)– Provide guidance for new practitioners– Promote method consistency– Increase reproducibility of results
![Page 9: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/9.jpg)
(2) ASTM D5744 DevelopmentWHAT?
Formalized, robust waste rock dissolution test method
WHY?
• Provide detailed description of protocol– Provide guidance for new practitioners– Promote method consistency– Increase reproducibility of results
WHO? Bill White (USBM, USBLM) retired
![Page 10: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/10.jpg)
(2) ASTM D5744 DevelopmentWaste Rock
OBJECTIVES1) Determine relative degrees of reactivity
2) Provide rates for modeling solute release in field
Does NOT simulate field drainage.
![Page 11: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/11.jpg)
(3) ASTM D5744 DescriptionStart to Finish
3.1 Rock sample to be tested
3.2 Laboratory test protocol
3.3 Post-test rock analysis
![Page 12: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/12.jpg)
(3.1) ASTM D5744Rock Sample to be Tested
• Collection: methods, amount• Storage• Preparation– Drying– Screening– Size reduction– Splitting
• Analysis
![Page 13: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/13.jpg)
(3.1) Sample PreparationCrushing
![Page 14: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/14.jpg)
(3.1) Sample PreparationSieving -1/4 inch
![Page 15: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/15.jpg)
(3.1) Sample PreparationSplitting
![Page 16: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/16.jpg)
(3.1) Sample PreparationCrushed splits for analysis
![Page 17: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/17.jpg)
(3.1) Rock Sample Analysis
• Particle size distribution• Chemistry– S, S2-, CO3, whole rock, trace element
• Mineral content & chemistry (e.g. carbonates)• Size fractions– S, S2-, CO3
– CO3
– AP, NP mineral liberation
![Page 18: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/18.jpg)
(3.1) Pyrite included: +2000 μm Archean greenstone rock
![Page 19: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/19.jpg)
(3.1) Partially exposed pyrite:75-150 μm Archean greenstone rock
![Page 20: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/20.jpg)
(3.1) Liberated pyrite: 75-150 um Archean greenstone rock.
![Page 21: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/21.jpg)
(3.1) Archean greenstone FeS2 oxidation rate: Observed/Predicted (Williamson & Rimstidt 1994).
![Page 22: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/22.jpg)
(3.2) ASTM D5744 Test Protocol1 kg Archean greenstone rock, d < 6.25 mm
![Page 23: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/23.jpg)
(3.2) ASTM D5744 Protocol
• Load cell, initial rinse (500 or 1000 mL)• Rock reacts with water air for 1 week• Controlled T, R.H.• Rinse on seventh day (500 or 1000 mL)• Determine drainage volume• Analyze drainage
![Page 24: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/24.jpg)
(3.2) ASTM D5744 ProtocolOption AAIRFLOW
• Set at 1-10 L/min ± 0.5 L/min• 3 day dry air (R.H. < 10%) – DO NOT DRY CELL COMPLETELY
• 3 day humidified air (R.H. ~95%)
![Page 25: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/25.jpg)
(3.2) ASTM D5744 Option A Array
![Page 26: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/26.jpg)
(3.2) ASTM D5744Option B
• No air flow
• Controlled T, R.H.
• More consistent and higher water content
• Enhanced acid neutralization for some rocks
![Page 27: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/27.jpg)
(3.2) ASTM D5744 Option B
![Page 28: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/28.jpg)
(3.2) ASTM D5744 Option B
![Page 29: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/29.jpg)
(3.2) ASTM D5744 Humidity Cell
• Dissolution test procedure– Apparatus– Solid addition to cell– Airflow– Reaction T, RH, water retention– Leachant• Volume• Quality
– Leachate analysis (solutes, frequency)
![Page 30: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/30.jpg)
(3.2) Uncontrolled Temperature[SO4] oscillates ~ factor of 10
![Page 31: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/31.jpg)
(3.2) Uncontrolled Temperature[SO4] oscillates ~ factor of 10
![Page 32: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/32.jpg)
(3.2) Controlled Temperature
![Page 33: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/33.jpg)
(3.2) Test Duration Dependent on Test Objectives.
• No prescribed duration
• Clearly define objectives with test design
• Examine data at regular intervals to see if objectives met.
• If (Ca + Mg)CO3 content high, determination of reactivity might require long test
![Page 34: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/34.jpg)
Data from different method used to demonstrate test duration.
![Page 35: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/35.jpg)
Test Duration: Time to acidification
![Page 36: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/36.jpg)
Test Duration: Time to acidification
![Page 37: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/37.jpg)
Test Duration: Time to acidification
![Page 38: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/38.jpg)
Test Duration: Time to acidification
![Page 39: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/39.jpg)
Test Duration: Time to acidification
![Page 40: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/40.jpg)
Test DurationDescribe Dissolution Behavior
DISCOVERY
How will rock dissolve?
![Page 41: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/41.jpg)
Minimum pH: saturated ~ 0.2-0.3 units lower than evaporating
![Page 42: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/42.jpg)
Max rates: dNi/dt (sat) ~ 20-25 dNi/dt (evap)
![Page 43: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/43.jpg)
(3.3) ASTM D5744Post-test rock analysis
• Visual examination
• Leach extractions
• Mineralogical examination
![Page 44: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/44.jpg)
![Page 45: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/45.jpg)
(4) Data Analysis
Kinetic test data contributions
4.1) Determine relative degrees of reactivity
4.2) Provide data to quantifying solute release rates
![Page 46: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/46.jpg)
(4) Data Analysis:(4.1) Reactivity Examples
• Waste rock lithology – negligible carbonate– S present as sulfide
• **KINETIC TEST PROGRAM DESIGN**
– Select multiple samples of variable S content
– Subject to long-term (kinetic) dissolution testing
– Compare results as f(%S)
![Page 47: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/47.jpg)
(4.1) Archean Greenstone: As S content increased: drainage pH decreased and [SO4]
increased. (“Reactivity” increases with S)
0 50 100 150 200 250Weeks
0
250
500
750
[SO
], u
mo l
/L
345678
pH
0 50 100 150 200 2500
250
500
750345678
pH
0 50 100 150 200 2500
250
500
750345678
pH0.05 %S
0.20 %S
0.20 %S
1.22 %S
4
![Page 48: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/48.jpg)
(4.1) Archean Greenstonemin pH (Reactivity) vs %S
154 – 204 week record
% S min pH
0.04 – 0.05 6.4 – 6.8
0.10 – 0.16 5.4 – 5.9
0.20 – 0.40 3.6 – 3.9
0.59 – 1.22 3.0 – 3.3 2
3
4
5
6
7
0 0.4 0.8 1.2
Min
imum
pH
% Sulfur
![Page 49: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/49.jpg)
(4.1) Minimum pH vs. %S (Reactivity)Informs waste rock management
Archean greenstone%S min pH Management0.04-0.05 6.4-6.8 Meets pH standards1
0.10-0.16 5.4-5.9 Slight pH adjustment?0.20-0.40 3.6-3.9 Substantial mitigation0.59-1.22 3.0-3.3 Rigorous mitigation1 Must check for potential problematic solutes
![Page 50: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/50.jpg)
(4.2) Troctolitic rock reactivity, min pH vs %S
2
3
4
5
6
7
0.0 0.5 1.0 1.5 2.0
Min
imum
pH
% Sulfur
324 – 726 week record
% S min pH
< 0.22 ~ 6.0
0.40 – 0.58 3.8 – 4.1
0.71 – 1.64 3.1 – 3.6
![Page 51: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/51.jpg)
(4.2) Data Analysis:Solute release rates
• Observed rates to determine field behavior
• Scale lab to field (NO SMALL TASK)
• Modeling to determine source terms
![Page 52: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/52.jpg)
(4.2) Data Analysis:Solute release rates
• Humidity cell test yields– Solute concentrations– Drainage volume
• Can calculate solute release rates– Statistical description of all weekly rates or– For periods of relatively constant release • Average release rate and• Standard deviation
![Page 53: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/53.jpg)
(4.2) Determine SO4 release ratesArchean Greenstone, 1.22% S
0 50 100 150 200 250Weeks
0
250
500
750
[SO
], u
mo l
/L
345678
pH
0 50 100 150 200 2500
250
500
750345678
pH
0 50 100 150 200 2500
250
500
750345678
pH0.05 %S
0.20 %S
0.20 %S
1.22 %S
4
![Page 54: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/54.jpg)
(4.2) Average sulfate rates: µmol(kg•wk)-1
0
100
200
300
400
0 50 100 150 200 250
dSO
4/d
t
Week
S.D. = 51
Avg = 292
S.D. = 31Avg = 226
![Page 55: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/55.jpg)
Summary
• ASTM D5744-13 detailed protocol[and 27 explanatory notes]
• Rigorous review process
• Approved in 1996, revised 2007, 2013
• Robust replication testing
![Page 56: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/56.jpg)
ASTM D5744-13 Humidity Cell
• Provide detailed description of protocol– Provide guidance for new practitioners– Promote method consistency– Increase reproducibility of results
• Contributes to environmentally sound management of mine wastes today
• Generates data to improve understanding of mine waste dissolution tomorrow.
![Page 57: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/57.jpg)
Helpful References
Method Description
ASTM International. 2013a. D5744-13, Standard test method for laboratory weathering of solid materials using a humidity cell. In Annual book of ASTM Standards, 11.04. American Society for Testing and Materials International, West Conschohocken, PA. 23 p. (http://www.astm.org/Standards/D5744.htm?A).
Bucknam. C.H., White III, W., Lapakko, K.A. 2009. Standardization of Mine Waste Characterization Methods by ADTI-MMS. In Proc. Securing the Future and 8thICARD, June 22-26, 2009, Skellefteå, Sweden (CD ROM). 12 p.
Lapakko, K.A. 2003. Developments in humidity cell tests and their applications. InEnvironmental Aspects of Mine Wastes, J.L. Jambor, D.W. Blowes, and A.I.M. Ritchie, Eds., Mineralogical Association of Canada Short Course Volume 31, 2003, p. 147-164.
To order method: [email protected]
![Page 58: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/58.jpg)
Helpful ReferencesRobustness Testing
Lapakko, K.A., White, W.W. III. 2000. Modification of the ASTM 5744-96 kinetic test. In Proceedings from the Fifth International Conference on Acid Rock Drainage.SME, Littleton, CO. p. 631-639.
Lapakko, K.A., White III, W.W. 2013. Research Report D34-1019: Interlaboratory study to establish precision statements for ASTM D5744-13, Test method for laboratory weathering of solid materials using a humidity cell. Committee D34 on Waste Management, Subcommittee D34.01.04 on Waste Leaching Techniques, 1 September 2013. ASTM International, 100 Barr Harbor Drive, West Conshohocken, PA 19428. 111 p. (D34-1019 available upon request through ASTM Customer Service at [email protected].)
White III, W.W., Lapakko, K.A. 2000. Preliminary indications of repeatability and reproducibility of the ASTM 5744-96 kinetic test for drainage pH and sulfate release rate. In Proceedings from the Fifth International Conference on Acid Rock Drainage. SME, Littleton, CO. p. 621-630.
![Page 59: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/59.jpg)
Helpful ReferencesSurface area available for reaction
Lapakko, K.A., Antonson, D.A. 2006. Pyrite oxidation rates from humidity cell testing of greenstone rock. In Proc. 2006, 7th ICARD, March 26-30, 2006, St. Louis MO. Published by ASMR, 3134 Montavesta Rd., Lexington, KY 40502. p. 1007-1025.
Lapakko, K. A., Engstrom, J.N., Antonson, D. A. 2006. Effects of particle size on drainage quality from three lithologies. In Proc. 2006, 7th ICARD, March 26-30, 2006, St. Louis MO. Published by ASMR, 3134 Montavesta Rd., Lexington, KY 40502. p. 1026-1050. http://www.imwa.info/docs/imwa_2006/1026-Lapakko-MN-2%20.pdf
![Page 60: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/60.jpg)
Helpful References
Test Duration
Lapakko, K. A., Berndt, M. 2009. Laboratory dissolution of tailings under three different test conditions. In Proc. Securing the Future and 8th ICARD, June 22-26, 2009, Skellefteå, Sweden (CD ROM). 11 p.
Lapakko, K. A., Wessels, J. N. 1995. Release of acid from hydrothermal quartz-carbonate hosted gold-mine tailings. In Sudbury '95, Conference on Mining and theEnvironment, Sudbury, Ontario, May 28th - June 1st, 1995. p. 139-148.
![Page 61: ASTM D5744 Kinetic Test Method Status and …bc-mlard.ca/files/presentations/2013-10-LAPAKKO-astm-d...ASTM D5744 Kinetic Test Method Status and Application Kim Lapakko kim.lapakko@state.mn.us](https://reader038.fdocuments.in/reader038/viewer/2022103107/5a831ca17f8b9a9d308e8741/html5/thumbnails/61.jpg)
Helpful References
Good Prediction References
Maest A.S., Kuipers, J.R., Travers, C.I., Atkins, D.A. 2005. Predicting water quality at hardrock mines: methods and models, uncertainties and state-of-the-art. Kuipers& Associates and Buka Environmental. http://www.ceaa-acee.gc.ca/050/documents_staticpost/cearref_3394/hearings/SM09.pdf
Morin, K., Hutt, N. Mines, Mining, and the Environment, Case studies. http://www.mdag.com