Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed,...

47
Manufacturing Consideration

Transcript of Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed,...

Page 1: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Manufacturing Consideration

Page 2: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Manufacturing Considerations

• Injection Molding is a high speed, automated process that can be used to produce simple to very complex parts

• The part designer must recognize that the design of the part determines the ease of molding, the tooling requirements and the cost

• Also the designer must recognize that the properties of the part are greatly affected by the mold design and processing conditions

Page 3: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Manufacturing Consideration

• Injection molding is a series of sequential process steps, each of which has an influence on the properties of the resultant part– Mold filling– Packing– Cooling– Ejection

Page 4: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Manufacturing Consideration

• Gating

• Orientation

• Pressure losses

• Frozen in stress

• Shrinkage and Warpage

• Weld/Meld lines

• Flow leaders/restrictors

Page 5: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Gating

• The gate is the melted plastics entry into the mold cavity

• Usually the thinnest cross section in the system• The gate type, number of gates and gate location

has a dramatic effect on overall part quality– Determines the mold filling pattern

– Induces shear and shear heating

– Affects shrinkage and warpage

Page 6: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Gating

• Gating determines the type and cost of the mold– Edge or sub gated parts can be produced with a

standard cold runner two plate mold– Top center gating or multiple top gating

required a three plate mold

Page 7: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Gate Design Rules

• Gate centrally to provide equal flow length

• Gate symmetrically to avoid warpage

• Gate into thicker sections for better filling and packing

• Gate long, narrow parts from an end for uniform flow

Page 8: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Gate Design Rules

• Position the gate away from load-bearing areas

• Hide the gate scar • Gate for proper weld-line location and

strong weld lines • Multiple gates shorten flow lengths• Locate gates on either side of a weak core

or insert

Page 9: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Orientation

• Almost all injection molded parts have some degree of frozen-in molecular orientation

• The degree is determined by the molecular weight, relaxation characteristics, and processing conditions

• Orientation greatly affects the properties of the part– Shrinkage– Strength– Residual stresses

Page 10: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Orientation

• Mold filling related orientation can be affected through process variables that affect mold filling pressure requirements– Flow direction and speed– Channel dimensions– Temperatures

• Residual Orientation = Orientation due to flow - relaxation

Page 11: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

How Molecular Orientation Occurs

• Molecular orientation develops during mold filling as the plastic is injected through the nozzles, runner, gate and cavity

• The polymer chains become stretched out due to velocity gradients

• The orientation tends to be in the direction of flow

Page 12: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

How Molecular Orientation Occurs

• The blunted shape of most polymer melt velocity profile causes most of the orientation to occur toward the surface.

• The molecules at the core remain random• Extreme in injection molding where the melt

adjacent to the cold mold will freeze first, leading to high interfacial shear stresses and not allowing for relaxation

• Problems are most significant for higher molecular weight plastics and fiber reinforced plastics

Page 13: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

How Molecular Orientation Occurs

Page 14: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Effects of Molecular Orientation

• Orientation creates different directional properties– Stronger is the flow direction– Weaker in the transverse direction

Page 15: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Effects of Molecular Orientation

• Typical directional property of an injected molded part

Page 16: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Orientation

• The degree of orientation caused by mold filling is influenced by processing conditions, material properties, mold design and part design– Large diameter runners, sprues, gates along

with shorter flow lengths will reduce orientation

– Faster fill rates and higher melt temperatures tend to promote molecular relaxation

Page 17: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Mold Filling Pressure Loses

• When selecting a gate location, it should be such that the mold fills uniformly, the pressure drop is not excessive and the shear rate does not exceed the limit of the polymer

• The designer must obtain an estimate of the pressure drop to evaluate the moldability of the part with respect to a proposed gating scheme

• The pressure drop depends on the material, mold and processing conditions

Page 18: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Mold Filling Pressure Loses

• Assuming isothermal, laminar, Newtonian fluid (ok for engineering estimate) the equations for pressure drop and shear rate are:

– Cylindrical Rectangular

3

2

*

***12*

*6

HW

LQP

HW

Q

4

3

*

***8*

*4

r

LQP

r

Q

r

L

W

H

L

Page 19: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Mold Filling Pressure Loses

is the shear viscosity– Pa-sec, lb-sec/in2

is the apparent wall shear rate– Sec-1

• Q is the volumetric flow rate– M3/s, ft3/s

Page 20: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Apparent vs Corrected Shear Viscosity

• Most viscosity data is of the form apparent shear viscosity at the wall as a function of wall shear rate and temperature

• If shear viscosity is described as apparent, it is not corrected for pseudo-plastic behavior

Page 21: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Apparent vs Corrected Shear Viscosity

• The corrected shear viscosity is– Cylinder Rectangle

])13(

4[

n

nat ]

)12(

3[

n

nat

indexlawpowern

ityvisapparent

ityvistrue

a

t

cos

cos

Page 22: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Estimating Pressure Drop

• Determine part volume

• Determine volumetric flow rate

• Determine apparent shear rate

• Determine apparent shear viscosity

• Determine true shear viscosity

• Determine pressure drop

Page 23: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Estimating Pressure Drop Example

• High impact polystyrene ruler– Sprue 0.313”diameter by 2” length– Runner 0.25”diameter by 2.25” length– Edge Gate 0.08”deep by 0.4”wide by 0.12” length– Cavity 0.1”deep by 1.5”wide by 6.03” length

• Single cavity

• 200 degree centigrade• 1.5 seconds fill time• n=1

Page 24: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Estimating Pressure Drop Example

• Determine part volume– Cylinder

• V = *r2 *L

– Rectangle• V = L*W*H

• Sprue 0.154in3

• Runner 0.110in3

• Edge Gate 0.004in3

• Cavity 0.905in3

Page 25: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Estimating Pressure Drop Example

• Determine volumetric flow rate– For single cavity mold

– QT=Qs=QR=QEG=QC

– QT=VT/tF

• VT is total volume = 1.173in3

• tF is fill time = 1.5 seconds

• QT=0.782in3/sec

Page 26: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Estimating Pressure Drop Example

• Determine apparent shear rate– Cylinder Rectangular

– Sprue 259/sec

– Runner 510/sec

– Edge Gate 1830/sec

– Cavity 312/sec

3*

*4

r

Q

2*

*6

HW

Q

Page 27: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Estimating Pressure Drop Example

• Determine apparent shear viscosity– From figure– Conversion factor

• Lb*sec/in2 = 6894.7 Pa*sec

• Sprue 320 Pa*sec 0.046lb*sec/in2

• Runner 270 Pa*sec 0.039lb*sec/in2

• Gate 180 Pa*sec 0.026lb*sec/in2

• Cavity 305 Pa*sec 0.044lb*sec/in2

Page 28: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Estimating Pressure Drop Example

Page 29: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Estimating Pressure Drop Example

• Determine true shear viscosity– Cylinder Rectangle

– n=1

• Sprue 0.046lb*sec/in2

• Runner 0.039lb*sec/in2

• Gate 0.026lb*sec/in2

• Cavity 0.044lb*sec/in2

])13(

4[

n

nat ]

)12(

3[

n

nat

Page 30: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Estimating Pressure Drop Example

• Determine pressure drop• Cylinder Rectangular

• Sprue 305 psi• Runner 716 psi• Gate 149 psi• Cavity 1650 psi• Total 2820 psi

4*

***8

r

LQP

3*

***12

HW

LQP

Page 31: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Frozen in Stress

• Molding factors, such as uneven part cooling, differential material shrinkage or frozen in flow stresses cause undesirable residual stress

• Residual stresses can adversely affect – Chemical Resistance– Dimensional stability– Impact and tensile strength

Page 32: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Shrinkage and Warpage

• Injection molding is used to produce parts with fairly tight dimensional tolerances

• Many plastics exhibit relatively large mold shrinkage values

• If a plastic exhibits uneven directional shrinkage, warpage will result

• Shrinkage is affected by the material, the mold, the part geometry and the processing conditions

Page 33: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Shrinkage and Warpage

• Parts with thick and thin wall sections can easily warp because the thick sections take longer to pack and cool, resulting in uneven shrinkage– When the part is ejected the thicker hotter

sections will continue to cool and shrink

Page 34: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

PVT Behavior of Plastics

• Plastics have a positive coefficient of thermal expansion and are highly compressible in the molten state

• Volume of any given mass will change with both temperature and pressure

• Semi-crystalline plastics shrink more than amorphous because of the ordered crystalline regions

Page 35: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

PVT Behavior

Page 36: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

PVT Behavior

Page 37: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Linear Mold Shrinkage

• Volumetric shrinkage can be predicted theoretically if PVT characteristics and the processing conditions

• We need linear shrinkage for cavity design– Linear Shrinkage = 1-(1-volumetric shrinkage)1/3

– Cavity dimension=Part dimension/(1-linear shrinkage)

– Expressed in in/in or mm/mm or %

Page 38: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Uneven Shrinkage and Warpage

• Uneven shrinkage is undesirable because it can lead to not hitting dimensions, internal stresses and warpage

• Main causes– Differential shrinkage due to orientation

– Differential cooling due to differences in cooling rate from cavity to core

– Cavity pressure differences due to too much pressure drop through the cavity

Page 39: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Mold Shrinkage Data

Page 40: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Mold Shrinkage Sample Problem

• The material that a part is made from has a volumetric shrinkage of 0.1in3/in3.

• What must be the cavity dimensions be to make a part– 3.02 inches wide– 5.67 inches long – 0.1 inches thick

Page 41: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Mold Shrinkage Sample Problem

in

inin

inThickness

in

inin

inLength

in

inin

inWidth

in

inS

S

SS

L

L

VL

104.00345.01

1.0

872.50345.01

67.5

128.30345.01

02.3

0345.0

)1.01(1

)1(1

3

1

3

1

Page 42: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Flow Leader and Restrictors

• Ideally the melt should flow from the gate, reaching the extremities of the cavity all at the same time

• To achieve balanced fill, the filling pressure drop associated with each and every flow path must be equal

• Pressure drops can be balanced by making local adjustments in the part wall thickness

Page 43: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Flow Leader and Restrictors

• Flow Leader are local increases in wall thickness to promote flow

• Flow restrictors are local decreases in wall thickness to reduce flow

• If flow is not balance– Overpacking/underpacking– Variable shrinkage– Residual Stress– Tendency to warp

Page 44: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Flow Leaders and Restrictors

Page 45: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Weld and Meld Lines

• Formed during filling when melt flow front separates and recombines

• Cause by– Multiple gates– Cores/Holes

• Looks like a crack on the surface of the part

Page 46: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Weld and Meld Lines

• The strength of the weld line can be significantly lower

• Try to eliminate completely or locate in non critical area in terms of load and appearance– Vary part geometry, part wall thickness and

gating scheme

Page 47: Manufacturing Consideration. Manufacturing Considerations Injection Molding is a high speed, automated process that can be used to produce simple to very.

Weld and Meld Lines

• Processing conditions affects the weld strength– Molecular diffusion and entanglement are

necessary to improve weld strength• Increase the temperature

• Increase the pressure