FHWA Update and Newest Advancements In Slurry Systems
Transcript of FHWA Update and Newest Advancements In Slurry Systems
![Page 1: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/1.jpg)
FHWA Update and Newest Advancements In Slurry Systems
Jason Dietz, Pavement & Materials Engineer
FHWA-OTS-RC
![Page 2: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/2.jpg)
FHWA Update - Every Day Counts (EDC-4) https://www.youtube.com/watch?v=qNXFD6LSoxo&feature=youtu.be&utm_content=&utm_medium=email&utm_source=govdelivery
![Page 3: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/3.jpg)
Benefits to Using a Whole-Life Approach to Pavement
Preservation Project and Treatment Selection
Pavement Preservation: When and Where
3
![Page 4: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/4.jpg)
States Requesting Assistance
4
CA
NV
OR
WA
ID
UT
AZNM
CO
WY
MT ND
SD
NE
KS
OK
TX LA
AR
MO
IA
MN
WI
IL
MS AL GA
TN
KY
IN
MI
OH
WVVA
NC
SC
PA
NY
FL
VT
NJ
CT
RI
MA
MENH
MD
DE
Alaska
Hawaii
DC
PR
VI
Requested Assistance
No Assistance Requested
No Response
FLH
![Page 5: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/5.jpg)
When and Where Program: Innovations
• Selection Guide
• Analysis Tool
• Peer-to-Peer Exchanges
• Communications Plan
• Asset Management
• Strategy Guidance
• Cost Effectiveness Metrics
https://www.fhwa.dot.gov/asset/pubs/life_cycle_planning.pdf
![Page 6: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/6.jpg)
EDC-4: Pavement Preservation When/Where• Implementation Plans (26 states)
• Web-based Training
• ISSA/FHWA Flexible (completed), Rapid Pavements (on-going)
• Federal-aid Essentials (on-going)
• Integrating Pavement Management to Selecting Pavements for Preventive Maintenance (1.5 Training)
• Provided (OK, LA, FL, MO, WA) 440 participants
• Upcoming (IL, NM, HI, PA, WI, AR)
• Peer Exchanges
Denver, CO (April 3-4, 2018)
Atlanta, GA (April 11-12, 2018)
Rocky Hill, CT (April 17-18, 2018)
![Page 7: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/7.jpg)
AASHTO Standards Developed or Under Development• Chip Seal – 2015
• Micro Surfacing – 2015
• Tack Coat – 2018
• Fog Seal – 2017
• Scrub Seal – 2018
• Sand Seal – 2018
• Slurry Seal – 2017
• Foam Asphalt Stabilization – 2018
• Thin Bonded Wearing Courses – 2018
• Cold Mixes• Virgin
• Recycled
• CIR - 2017
7
![Page 8: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/8.jpg)
Newest Advancements In Slurry Systems
![Page 9: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/9.jpg)
Slurry Seals are applied at onestone thickness.Typically 12-16 lbs/yd2
Micro Surfacing applied atmulti-stone thickness.Typically 25-30 lbs/yd2
![Page 10: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/10.jpg)
A Picture Is Worth a Thousand WordsLet’s set the stage, imagine a road 4 years old in good shape with no cracks. It only has slight to moderate chain wear, snow tire wear rutting in wheel paths, and 7,000 ADT. Now imagine that one lane is Slurry Sealed, the other lane is Micro Surfaced and a control section untouched. What does it look like 6 years later?
![Page 11: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/11.jpg)
Micro SurfacingSlurry Seal
No maintenance for
6 years
![Page 12: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/12.jpg)
Close up with straight edge looks like Pavement Preservation is paying off after 6 years
Micro SurfacingSlurry Seal
![Page 13: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/13.jpg)
NCAT Pavement Test Track
Lee Road 159
US-280
![Page 14: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/14.jpg)
Track Research Goals• Help state DOTs implement positive change
• Promote real innovation for the industry.
• Track Research overview
• Track preservation (APT)
• Lee Road 159 (low ADT)
• 2015 research cycle (high ADT)
![Page 15: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/15.jpg)
So what can we take away from the findings?
• Chip seal
• Scrub seal
• Scrub Cape seal
• Micro surface
• Thinlay
• Thinlay Scrub Cape seals.
15
![Page 16: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/16.jpg)
Benefits of Preservation
• Life extending benefit
• Condition improving benefit
• f (pretreatment condition)
![Page 17: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/17.jpg)
What is new in Polymer Modification in Asphalt Emulsions?• Typically anything over 4% polymer is very sticky and hard
to work with.
• Hard to emulsify SBR, and with SBS latex the chemistry of the latex starts to override set and break times of the emulsion.
• Performance from lab to field is very different.
![Page 18: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/18.jpg)
The MSCR TEST is Critical to early performance in power steering burns and long term durability from snow plows as seen in the next slides.
Specification
Hi- Mod Emulsion
Property Test
Procedure
(AASHTO)
Specification
Min Max
Asphalt Base Properties
Original DSR, kPa (G*/sin δ, 10 rad./sec)
@ 76°C
T315 1.00
Emulsion Properties
Viscosity, Saybolt-Furol, @ 122°F, SFS T59 15 150
Sieve Test, % T59 0.1T59 0.1
Residue by Evaporation, % T59 62T59 62
Residue Properties From Low
Temperature Evaporation
PP72-11, Procedure B
MSCR @ 70°C, Recovery @ 3.2 kPa, %TP70 80
Jnr @ 3.2/kPaTP70 0.50
![Page 19: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/19.jpg)
Hi-Mod Slurry Seal and Micro Surfacing
Multiple Stress Creep Recovery What is it? and how does it Help?
![Page 20: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/20.jpg)
Recoverable
Strain – 100%
How an Elastic Material Behaves
![Page 21: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/21.jpg)
DSR Test will indicate the presence of a polymer
Elastic Recovery Test
![Page 22: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/22.jpg)
Temperature
Softening PointASTM D36
![Page 23: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/23.jpg)
Material Testing Terms
Strain
Stress
Pascal
Jnr
Need to understand these terms…
![Page 24: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/24.jpg)
Strain is the response of a material to a stress along with the relative change in shape or size of an object as a result of a stress
Stress is the internal force per area associated with a stress and has the same units as pressure
Pascal – N/m2 – Pressure and Stress unit of measurement equal to 0.000145 PSI
Jnr = Unrecovered Shear Strain/Applied Shear Stress
![Page 25: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/25.jpg)
Multiple Stress Creep Recovery (MSCR)
What does MSCR mean?
… test method is used to identify the presence of elastic response in a binder and the change in elastic response at two different stress levels. Non-recoverable creep compliance has been shown to be an indicator of the resistance of an asphalt binder to permanent deformation under repeated load.
![Page 26: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/26.jpg)
Used to determine polymer in the AC/elastomeric properties. Material tested at two different stress levels, 1 second strain, 9 second recovery time for ten cycles
100 Pascals
Jnr
% Recovery
3200 Pascals
Jnr
% Recovery
% Difference between Jnr at 100 Pascals and 3200 Pascals
Graph of Jnr vs % Recovery at 3200 Pascals
MSCR
Time seconds40
MSCR
![Page 27: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/27.jpg)
2 4 6 8 10 12
1
2
3
4
5
6
7
gr = recovered strain
gu = un-recovered strain
gp = Peak strain
gp X 100r /g% recovery=
time s
stra
in
Plot showing the determination of the % recovery in the MSCR test
One Cycle in Detail
![Page 28: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/28.jpg)
Power Steering Burn Test. Five turns to left and five turn to the right• Conventional Micro on the Left Vs Hi-Mod and Micro is on the right. • Same rock, both down for 11 months.• Temp 93F air, surface temp 120F
![Page 29: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/29.jpg)
Type II Slurry Type II Hi-Mod Slurry
Below we have a side by side comparison of CQS-1H vs. CQS Hi Mod . The power steering burn on the CQS is greater than the Hi-Mod. The Hi-Mod is more of a scuff than a tear to the base.
Victorville, California 08/11/2015 one week after lay down.
![Page 30: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/30.jpg)
La Quinta, CA near Palm Springs ComparisonThe traditional Slurry is tearing and the other is scuffing. After one
week of service, 90% reduction in power steering burns in cul-de-sac.
Type II Slurry 2.5% polymer Hi -Mod Type II Slurry
![Page 31: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/31.jpg)
Cul-de-sac done with conventional LMCQS-1h, not Hi-Mod
![Page 32: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/32.jpg)
Adjacent cul-de-sac done with Hi-Mod
![Page 33: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/33.jpg)
Hi-Mod Emulsion for Slurry Seals & Micro Surfacing• An innovative new product (high
polymer content) which is much tougher than its conventional counterparts–Higher temperature tolerant to reduce
scuffing and tearing
–More damage resistant to resist snow plowing
33
![Page 34: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/34.jpg)
Expectations
Verification: Contabro Test
On The Road: Demonstrations/Projects
![Page 35: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/35.jpg)
CANTABRO LOSSScope
• This test method determines the abrasion loss of compacted slurry, micro and hi-mod micro samples.
• Measures the breakdown of various emulsion specimens utilizing the Los Angeles Abrasion machine
![Page 36: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/36.jpg)
Test ProcedureMold specimens• Oven dry specimens in an oven until cured, not exceeding 24 hours.
Temperature of oven shall be no greater than 140 F and not less than 122 F. Weigh specimen and record as A.
• Place individual specimen in the Los Angeles testing machine. (do not include steel balls)
• Rotate the machine at a speed of 30-33 rpm’s for 300 revolutions. After 300 revolutions, discard any loose material broken off of the specimen.
• Weigh the specimen record as B
![Page 37: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/37.jpg)
Calculation
Use the following formula to measure Cantabro Loss:CL = A - B
A
CQS-1H MICRO HI-MOD MICRO
Mass Loss % = 2.89 Mass Loss % = 0.04 Mass Loss % = 5.21
![Page 38: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/38.jpg)
#3 Hi-Mod Type III
#2 Micro Type III
#1 Conventional Slurry Seal
Type III
1
Cantabro Testing Type III ISSA Micro Surfacing Gradation after 300 revolutions
![Page 39: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/39.jpg)
![Page 40: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/40.jpg)
WHY USE Hi-Mod EmulsionsThe Performance:This is the toughest emulsion that can be specified for these categories. It can handle the early damage. • Project selection is the same as any other Micro or Slurry seal
project. • Mix design is the same.• Inspection is the same.• Emulsion Specification is different. • Construction is slightly different as the contractor must use an
augured box due to the higher viscosity of the mix, i.e. much thicker.
![Page 41: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/41.jpg)
The MSCR TEST is Critical to early performance in power steering burns and long term durability.
Specification
CSS-1EP
Property Test
Procedure
(AASHTO)
Specification
Min Max
Asphalt Base Properties
Original DSR, kPa (G*/sin δ, 10 rad./sec) @
76°C
T315 1.00
Emulsion Properties
Viscosity, Saybolt-Furol, @ 122°F, SFS T59 15 150
Sieve Test, % T59 0.1T59 0.1
Residue by Evaporation, % T59 62T59 62
Residue Properties From Low Temperature
Evaporation
PP72-11, Procedure B
MSCR @ 70°C, Recovery @ 3.2 kPa, %TP70 80
Jnr @ 3.2/kPaTP70 0.50
![Page 42: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/42.jpg)
Must use an augured box with Hi Mod emulsions
![Page 43: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/43.jpg)
“We are confident Hi-Mod will extend service life by a couple of years over
conventional micro surfacing, making it a more cost-effective
process for the end users.”
RICHARD GOODICK VICE PRESIDENT,
SEALCOATING, INC.
![Page 44: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/44.jpg)
➢ The typical cost increase to use the Hi-Mod emulsion is .20 to .29 cents more per yd2.
➢ The expected life increase should be 3 or more years longer than your current Slurry and Micro products.
➢ Like all Slurry Seal and Micro Surfacing projects you should crack fill before application.
➢ Many contractors have seen and expect to observe 75% reduction in raveling and post project sweeping.
![Page 45: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/45.jpg)
Massachusetts Connecticut
Texas Big Bear California
![Page 46: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/46.jpg)
What are we working on in the lab?Crack Resistance
Texas Overlay Tester
13.5% Emulsion Content
0
20
40
60
80
100
120
140
160
Slurry Micro eFlex CR
Cyc
les
to F
ailu
re
Micro Surfacing Overlay Test
Type 2
Type 3
![Page 47: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/47.jpg)
Crack Resistance testing update after 14 Months all Cracks reflected back much better then control which was 4 Months all
crack wear back but not good enough still working on it.
14 Months AfterBefore 6 Months After
![Page 48: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/48.jpg)
Victorville, California• Hi-Mod was applied to residential streets in Victorville, California on July 31st, 2015.• Surface temperatures reached 1090F with air temps hitting 940F.• Aggregate was Vulcan, Highland Type II.
![Page 49: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/49.jpg)
Ground Tire Rubber In Slurry Seal & Micro SurfacingIncorporation Process
• 5% by weight of emulsion added at machine through fines feeder.
• 5% blended into the aggregate.
• 5% GTR Terminal Blended in the asphalt and then emulsified.
• Meets recycling credits.
• No mix performance benefits have ever been proven.
• Greater then 5% we have seen problems with raveling in all processes.
• Due to compression and or moisture resistance.
Benefit
![Page 50: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/50.jpg)
Ground Tire Rubber in Slurry Seal and Micro Surfacing (cont.)Construction
• Recommend that you specify and use a rubber tire roller to roll the section to reduce raveling.
• Using very fine 30 to 80 mesh ground tire rubber.
• How to verify the amount of rubber being used ??
Ground Tire Rubber
![Page 51: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/51.jpg)
Ground Tire Rubber Blended into Type II Slurry Aggregate30 mesh ground tire rubber Blended agg with 5% GTR
5% GTR
+ =
100 grams105 grams Blend Material
![Page 52: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/52.jpg)
Truck Added GTRGround Tire Rubber GTR
• The GTR is being added through an extra fines feeder. That is mounted on the machine.
![Page 53: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/53.jpg)
City of Ontario Ca Using Tire Rubber Slurry
“RPMS”
![Page 54: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/54.jpg)
100,000 pound
Tire Rubber Silo
Mix Tank
Processing Vessel
Rotary Valve
Processing Pumps
Tire Rubber is fed Pneumatically
The GTR is Digested into Asphalt at Processing Plant then emulsified into a Slurry Seal or Micro Surfacing emulsions.
Terminal BlendedGround Tire Rubber
![Page 55: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/55.jpg)
TRMSS Emulsion Place as Slurry Seal orMicro Surfacing
1.
![Page 56: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/56.jpg)
City of Port Hueneme CAUsing RAP Aggregate with Hi-Mod Micro Surfacing Emulsions
![Page 57: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/57.jpg)
Milling is the best source of RAP
![Page 58: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/58.jpg)
Cost: Utilization of 100% RAP Chip and Slurry Seal
Crushing Utilization Concerns
• Average breakdown
✓Chip Seal 45%
✓Slurry Dust 50%
✓Other 5%
![Page 59: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/59.jpg)
Utilization
Solution
Utilize the source for the most productive product
Produce multiple products if possible
![Page 60: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/60.jpg)
Best Practices• Slurry Seal
• RAP Fines must be fresh. Material that has been stored or stockpiled too long should be re-screened.
• Stock Pile Management
• Do not stock pile too much material
• Use material as it is delivered (load out from all sides)
• Do not load trucks the night before
• Minimum requirement of 3% latex polymer
• Rubber tire roller, minimum three passes
• High traffic areas can not be over asphalted
![Page 61: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/61.jpg)
Utilization of 100% RAP Chip & Slurry Seal
• Recycled Products are Valuable.
• Recycled Pavement Preservation
Processes are performing great.
• Increased Utilization will Reduce
Cost.
• We Need Industry Help to Protect
Resources.
![Page 62: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/62.jpg)
Do Agencies Know About This?
![Page 63: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/63.jpg)
What questions do you have?
Pavement & Materials Technical Service Team
![Page 64: FHWA Update and Newest Advancements In Slurry Systems](https://reader031.fdocuments.in/reader031/viewer/2022012022/6169c81311a7b741a34b4b0e/html5/thumbnails/64.jpg)
For more information: